Method for recycling and reusing PET core material of wind power blade

By peeling, cutting, and controlling the reaction conditions of the surface skin of the PET core material of wind turbine blades, unsaturated polyester resin is synthesized, solving the problem of PET core material recycling and realizing efficient reuse and environmentally friendly industrial applications.

CN119019616APending Publication Date: 2024-11-26SWANCOR ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411048843.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing technology has limited recycling methods for PET core materials for wind turbine blades, making it difficult to reuse them, and their waste is harmful to the environment.

Method used

A method for recycling and reusing PET core material is provided, including peeling off the surface skin, cutting, weighing raw materials in proportion, and reacting in a filtration device under controlled temperature and time to synthesize unsaturated polyester resin.

Benefits of technology

This technology enables the efficient recycling and reuse of PET core materials for wind power. The synthesized unsaturated polyester resin has excellent mechanical properties, making it suitable for industrial production and application, and reducing carbon dioxide emissions and pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019616A_ABST
    Figure CN119019616A_ABST
Patent Text Reader

Abstract

The invention provides a method for recovering and reusing a PET core material. The method comprises the following steps: stripping a skin, degrading the PET core material, separating thermosetting resin, preparing unsaturated polyester resin from a degradation product and the like. Belongs to the technical field of resin materials. The unsaturated polyester resin is synthesized by utilizing the recycled wind power PET core material, the preparation process is simple, the wind power PET core material waste can be converted into a product with higher economic value, the unsaturated polyester resin is beneficial to reducing carbon dioxide emission and reducing pollution, and the unsaturated polyester resin synthesized based on the recycled PET core material has excellent mechanical properties and is suitable for industrial production. The tensile strength is 50-70 MPa, the bending strength is 100-130 MPa, the elongation at break is 3-5%, and the material is suitable for industrial production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for recycling and reusing a PET core material, belonging to the technical field of resin materials. Background Art

[0002] PET is a semi-crystalline thermoplastic polyester with excellent chemical stability, tensile and impact strength, as well as light weight, transparency and low gas permeability. However, the synthetic raw materials of PET come from non-renewable petroleum resources, and it takes hundreds of years to decompose in the natural environment. Its microparticles easily accumulate in organisms and harm the ecology. In addition, PET waste is a carrier of toxic colorants and additives. Therefore, recycling PET for reuse has far-reaching significance in terms of resource conservation and environmental protection.

[0003] Wind power generation is a renewable and sustainable energy source, and it is also a clean energy source without carbon dioxide emissions. However, from the perspective of its impact on the environment throughout its life cycle, the energy consumption and process flow in the production of wind power components will generate a large amount of carbon dioxide, and a lot of waste will be generated at the end of its life cycle. In order to improve the environmental benefits of wind power generation throughout its life cycle, the efficient recycling of wind power waste has become a focus of attention. Wind turbine blades are a composite structure, usually composed of reinforcing fibers, polymer matrix, foam sandwich materials, coatings and metals. Among them, one of the most common materials in foam sandwich materials is PET core material. Due to the complex structure of wind turbine blades and the residual thermosetting resin (such as epoxy resin and unsaturated polyester resin) in the PET groove, the recycling of PET core material is more complicated than the recycling of PET bottle waste. Therefore, there are few studies on the recycling of PET core material. However, considering that a large number of wind turbine blades will be retired in the near future, there is a considerable demand for wind power material recycling technology. Therefore, research on the recycling and reuse of PET core material of wind turbine blades is of great significance.

[0004] Therefore, there is an urgent need in the art for a method for recycling and reusing the PET core material of wind turbine blades. Summary of the invention

[0005] The purpose of the present invention is to solve the problem of limited recycling methods of PET core materials of wind turbine blades in the prior art.

[0006] In order to achieve the purpose of solving the above problems, the technical solution adopted by the present invention is to provide a method for recycling and reusing PET core material, comprising the following steps:

[0007] Step 1: After peeling off the surface skin, cut the remaining PET core material into suitable sizes for later use;

[0008] Step 2: Weigh various raw materials according to the formula ratio, including:

[0009] PET core material: 15% ~ 25%;

[0010] Diol monomer: 25% to 30%;

[0011] Antioxidant: 0.01%~0.04%;

[0012] Catalyst: 0.01%~0.05%;

[0013] Reagents that inhibit free radical reactions: 0.01% to 0.05%;

[0014] Unsaturated dibasic acid: 10% to 25%;

[0015] Saturated dibasic acid: 0-15%;

[0016] Reactive diluent monomer: 25% to 35%;

[0017] Each percentage is by mass;

[0018] Step 3, the diol monomer, antioxidant and catalyst in step 2 are added into a reactor with a filtering device, and the PET core material is added in batches according to the volume of the reactor, and the temperature is maintained at 190-250° C. for 1-2 hours each time, and then the temperature is lowered to 50° C., the thermosetting resin that does not participate in the reaction is filtered out, and the PET core material is continued to be added, and the above operation is repeated until all the PET core material is added and reacted completely. After the reaction is completed, the filtrate is collected and the next step is carried out;

[0019] Step 4: Evenly mix the above-mentioned degradation filtrate with the inhibitor, the unsaturated dibasic acid and the saturated dibasic acid, and keep the reaction at a temperature of 190-220°C for 10-24 hours. During this process, the carboxylic acid and the alcohol undergo a polycondensation reaction, the acid value of the reactant decreases, and the viscosity increases. The reaction end point can be set according to demand. The acid value of the reactant and the viscosity at 150°C are measured every 0.5-1 hour. If the acid value is <24 and the viscosity is >350cps, the reaction end point is reached. Then cool to below 100°C, add a reactive diluent monomer to terminate the reaction, and the resulting finished product is an unsaturated polyester resin prepared based on recycled PET core material.

[0020] Preferably, in step 2, the proportion of the thermosetting resin contained in the PET core material accounts for 30-50% of the entire core material.

[0021] Preferably, in step 2, the diol monomers include ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, neopentyl glycol, 2,2,4-trimethyl-1,3-pentanediol, 1,4-cyclohexanedimethanol, bisphenol-A polyoxypropylene ether and dibromoneopentyl alcohol.

[0022] Preferably, in step 2, the antioxidant includes phosphoric acid, triphenyl phosphate, trimethyl phosphate, triethyl phosphoacetate, phosphites and hindered phenols.

[0023] Preferably, in step 2, the catalyst includes Mn(OAc)2, Co(OAc)2, Cu(OAc)2, Ni(OAc)2, monobutyltin oxide, titanium phosphate, Na2CO3, NaHCO3, Na2SO4, K2SO4, zeolite, Mn3O4 / SNPs and Fe3O4-MWCNT.

[0024] Preferably, in step 2, the reagents for inhibiting free radical reactions include quinones, hydroquinones, phenols, polyphenols, organic and inorganic copper salts, amines and nitro compounds; and the unsaturated dibasic acids include maleic anhydride and fumaric acid.

[0025] Preferably, in step 2, the saturated dibasic acid includes phthalic anhydride, isophthalic acid, terephthalic acid, adipic acid, glutaric acid and azelaic acid.

[0026] Preferably, in step 2, the reactive diluent monomers include monomers of styrene, α-methylstyrene, vinyltoluene, dicyclopentadiene acrylate, 4-chloromethylstyrene, acrylic acid, methyl acrylate, methacrylic acid, methyl methacrylate, glycidyl methacrylate, glycidyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, divinylbenzene and tripropylene glycol diacrylate.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1) The present invention utilizes recycled wind power PET core material to synthesize an unsaturated polyester resin, which has a simple preparation process and can convert wind power PET core material waste into products with higher economic value, which is beneficial to reducing carbon dioxide emissions and reducing pollution.

[0029] 2) The unsaturated polyester resin synthesized based on the recycled PET core material of the present invention has excellent mechanical properties, a tensile strength of (50-70) MPa, a flexural strength of (100-130) MPa, and an elongation at break of (3-5)%, and is suitable for industrial production and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The infrared spectra images of the PET degradation products and the synthesized unsaturated polyester resin in Example 1 are shown. DETAILED DESCRIPTION

[0031] In order to make the present invention more clearly understood, a preferred embodiment is described in detail with reference to the accompanying drawings as follows:

[0032] The invention provides a method for recycling and reusing PET core material.

[0033] Example 1

[0034] The synthesis method of unsaturated polyester resin based on recycled PET core material comprises the following steps:

[0035] Step 1: After peeling off the surface skin, cut the remaining PET core material into suitable sizes for later use.

[0036] Step 2, prepare the following components in parts by weight: a. PET core material A, PET content 66wt%: 19.10%; b. diol monomer: 28.59%; c. antioxidant: 0.02%; d. catalyst: 0.02%; e. inhibitor: 0.01%; f. maleic anhydride: 12.11%; g. phthalic anhydride: 14.02%; h. reactive diluent monomer: 26.13%.

[0037] Step 3, add diol monomer (12.64 parts of propylene glycol + 15.95 parts of diethylene glycol), antioxidant (0.02 parts of triphenyl phosphate), catalyst (0.02 parts of monobutyl tin oxide) into a reactor with a filtering device, and add a total of 19.10 parts of recycled PET core material in batches according to the volume of the reactor, keep the temperature at 230°C for 1 hour each time, then cool to 50°C, filter out the thermosetting resin that does not participate in the reaction, and continue to add PET core material, repeat the above operation until all the PET core material is added and reacted completely, collect the filtrate after the reaction and proceed to the next step.

[0038] Step 4: Evenly mix the above PET core material degradation filtrate with an inhibitor (0.01 parts of p-tert-butylcatechol), 12.11 parts of maleic anhydride and 14.02 parts of phthalic anhydride, and keep the reaction at 210°C for 14 hours, then cool to below 100°C, add a reactive diluent monomer (26.13 parts of styrene) to terminate the reaction, and the resulting product is an unsaturated polyester resin prepared based on the recycled PET core material.

[0039] The infrared spectra of the PET degradation products and the synthesized unsaturated polyester resin in Example 1 are as follows: Figure 1 shown.

[0040] Among them, in the infrared spectrum of PET degradation products, 3350cm -1 is the stretching vibration of OH, 2930, 2870cm -1 1120 cm-1 is attributed to the stretching vibration of CH3 and CH2 in terephthalate. -1Nearby is the superposition of antisymmetric and symmetric stretching vibrations of ether COC in the diethylene glycol structure. In summary, the degradation products of PET mainly include terephthalic acid glycol ester and unreacted monomer diol.

[0041] In the infrared spectrum of the synthesized unsaturated polyester resin, no characteristic peaks of OH groups appear, indicating that the diol is completely esterified. -1 Nearby is the out-of-plane bending vibration of the CH on the benzene ring of phthalic acid diol ester, 728cm -1 Nearby is the out-of-plane bending vibration of CH on the benzene ring of terephthalate; 1260cm -1 、1070cm -1 1629cm -1 The vicinity is C=C stretching vibration, indicating that maleic anhydride participates in the formation of the product resin. -1 、2956cm -1 A series of weak peaks nearby include the symmetric and antisymmetric stretching vibrations of CH3 and CH2, 1120 cm -1 Nearby is the superposition of the stretching vibration bands of COC in diethylene glycol. In summary, the synthetic end product is an unsaturated polyester obtained by polycondensation of propylene glycol, diethylene glycol, maleic anhydride, phthalic anhydride and terephthalic acid.

[0042] Example 2

[0043] The synthesis method of unsaturated polyester resin based on recycled PET core material comprises the following steps:

[0044] Step 1: After peeling off the surface skin, cut the remaining PET core material into suitable sizes for later use.

[0045] Step 2, prepare the following components by weight fraction: a. PET core material A, PET content 66%: 23.87%: b. diol monomer: 26.10%; c. antioxidant: 0.02%; d. catalyst: 0.02%; e. inhibitor: 0.01%; f. maleic anhydride: 11.05%; g. phthalic anhydride: 12.80%; h. reactive diluent monomer: 26.13%.

[0046] Step 3, add diol monomer (11.54 parts of propylene glycol + 14.56 parts of diethylene glycol), antioxidant (0.02 parts of triphenyl phosphate), catalyst (0.02 parts of monobutyl tin oxide) into a reactor with a filtering device, and add a total of 23.87 parts of recycled PET core material in batches according to the volume of the reactor, keep the temperature at 230°C for 2 hours each time, then cool to 50°C, filter out the thermosetting resin that does not participate in the reaction, and continue to add PET core material, repeat the above operation until all the PET core material is added and reacted completely, collect the filtrate after the reaction and proceed to the next step.

[0047] Step 4: Evenly mix the above PET core degradation filtrate with an inhibitor (0.01 parts of p-tert-butylcatechol), 11.05 parts of maleic anhydride and 12.80 parts of phthalic anhydride, and keep the reaction at 210°C for 14 hours, then cool to below 100°C, add a reactive diluent monomer (26.13 parts of styrene) to terminate the reaction, and the resulting product is an unsaturated polyester resin prepared based on the recycled PET core material.

[0048] Since the thermosetting resin will also degrade under the action of a catalyst at a temperature above 200°C, the present invention controls the reaction time and adds a filtering device to separate the thermosetting resin from the reaction system of alcohol and PET, and finally achieves the effect of successfully degrading PET while retaining the thermosetting resin as a whole. In the embodiment, since a filtering device is added and the temperature is lowered after the PET is completely dissolved, the thermosetting resin in the filter screen is separated from the reaction system in time, avoiding the degradation or swelling and dissolution of the thermosetting resin at high temperature and affecting the reaction.

[0049] Comparative Example 1

[0050] The difference from Example 1 is that a common reactor without a filtering device is used for the reaction, and no cooling and filtering operations are performed during the reaction. Since the thermosetting resin is not separated and filtered during the reaction, the thermosetting resin degrades and swells and dissolves at high temperature, completely absorbing the reacted diol monomer, resulting in reaction failure.

[0051] Comparative Example 2

[0052] The difference from Example 1 is that after the reaction reaches the end point, a reactive diluent monomer (26.13 parts of styrene) is added at 130° C. to terminate the reaction. Since the dilution operation is not performed within the temperature range required by the present invention, styrene self-polymerization induces system gelation and the reaction fails.

[0053] Comparative Example 3

[0054] The difference from Example 2 is that the reaction time of each batch of PET core material at 230° C. is shortened to 1 h.

[0055] Comparative Example 4

[0056] The difference from Example 2 is that the proportion of PET in the recycled PET core material is 70%.

[0057] Application Example 1

[0058] The molecular weight and polydispersity coefficient of the unsaturated polyester resins prepared in Examples 1 and 2 and Comparative Examples 3 and 4 are shown in Table 1.

[0059] Table 1 Pure resin molecular weight and polydispersity coefficient of Examples 1, 2 and Comparative Examples 3, 4

[0060] Example 1 Example 2 Comparative Example 3 Comparative Example 4 Number average molecular weight 1420 1444 1247 1367 Polydispersity coefficient 2.9794 2.239 2.723 2.880

[0061] Application Example 2

[0062] The mechanical properties of unsaturated polyester resins prepared by Examples 1 and 2 and Comparative Examples 3 and 4 were measured (pure resin casting body plate, 4 mm). The test results are shown in Table 2

[0063] Table 2 Mechanical properties of pure resin cast bodies of Examples 1, 2 and Comparative Examples 3, 4

[0064]

[0065] It can be seen from the data in Tables 1 and 2 that, compared with Comparative Example 3, Example 1 has a higher tensile strength. This is because the ratio of the PET core material to the diol monomer in the synthesized unsaturated polyester resin (66.81%) is smaller than that of Comparative Example 3 (91.46%), the PET core material is more thoroughly degraded, and the molecular weight of the synthesized unsaturated polyester resin (1420) is larger than that of Comparative Example 3 (1247); compared with Comparative Example 4, Example 2 has a higher tensile strength. This is because the extended degradation time also causes a higher degree of degradation of the PET core material. The molecular weight of the obtained unsaturated polyester resin (1444) is larger than that of Comparative Example 4 (1367), and the polydispersity coefficient of Example 2 is smaller (2.239), and the molecular weight distribution is more concentrated.

[0066] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and equivalent changes made by using the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for recycling and reusing PET core material, It is characterized in that The following steps are involved: Step 1: After peeling off the surface skin, cut the remaining PET core material into suitable sizes for later use; Step 2: Weigh various raw materials according to the formula ratio, including: PET core material: 15% ~ 25%; Diol monomer: 25% to 30%; Antioxidant: 0.01%~0.04%; Catalyst: 0.01%~0.05%; Reagents that inhibit free radical reactions: 0.01% to 0.05%; Unsaturated dibasic acid: 10% to 25%; Saturated dibasic acid: 0-15%; Reactive diluent monomer: 25% to 35%; Each percentage is by mass; Step 3, the diol monomer, antioxidant and catalyst in step 2 are added into a reactor with a filtering device, and the PET core material is added in batches according to the volume of the reactor, and the temperature is maintained at 190-250° C. for 1-2 hours each time, and then the temperature is lowered to 50° C., the thermosetting resin that does not participate in the reaction is filtered out, and the PET core material is continued to be added, and the above operation is repeated until all the PET core material is added and reacted completely. After the reaction is completed, the filtrate is collected and the next step is carried out; Step 4: Evenly mix the filtrate obtained in step 3 with the inhibitor, unsaturated dibasic acid and saturated dibasic acid, and keep the reaction at a temperature of 190-220°C for 10-24 hours. During this process, the carboxylic acid and alcohol undergo a polycondensation reaction, the acid value of the reactant decreases, and the viscosity increases. The reaction end point can be set according to demand. The acid value of the reactant and the viscosity at 150°C are measured every 0.5-1 hour. If the acid value is <24 and the viscosity is >350cps, the reaction end point is reached. Then cool to below 100°C, add a reactive diluent monomer to terminate the reaction, and the resulting finished product is an unsaturated polyester resin prepared based on recycled PET core material.

2. The method for recycling and reusing the PET core material according to claim 1, It is characterized in that In the step 2, the PET core material contains a thermosetting resin, the proportion of which accounts for 30-50% of the entire core material.

3. The method for recycling and reusing the PET core material according to claim 1, It is characterized in that In the step 2, the diol monomers include ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, neopentyl glycol, 2,2,4-trimethyl-1,3-pentanediol, 1,4-cyclohexanedimethanol, bisphenol-A polyoxypropylene ether and dibromoneopentyl alcohol.

4. The method for recycling and reusing the PET core material according to claim 1, It is characterized in that In the step 2, the antioxidant includes phosphoric acid, triphenyl phosphate, trimethyl phosphate, triethyl phosphoacetate, phosphites and hindered phenols.

5. The method for recycling and reusing the PET core material according to claim 1, It is characterized in that In the step 2, the catalyst comprises Mn(OAc) 2 、Co(OAc) 2 、Cu(OAc) 2 、Ni(OAc) 2 , monobutyltin oxide, titanium phosphate, Na 2 CO 3 、NaHCO 3 、Na 2 SO 4 , K 2 SO 4 , zeolite, Mn 3 O 4 / SNPs and Fe 3 O 4 -MWCNT.

6. The method for recycling and reusing PET core material according to claim 1, It is characterized in that In step 2, the reagents for inhibiting free radical reactions include quinones, hydroquinones, phenols, polyphenols, organic and inorganic copper salts, amines and nitro compounds; and the unsaturated dibasic acids include maleic anhydride and fumaric acid.

7. The method for recycling and reusing PET core material according to claim 1, It is characterized in that In the step 2, the saturated dibasic acid includes phthalic anhydride, isophthalic acid, terephthalic acid, adipic acid, glutaric acid and azelaic acid.

8. The method for recycling and reusing PET core material according to claim 1, It is characterized in that In the step 2, the reactive diluent monomers include monomers of styrene, α-methylstyrene, vinyltoluene, dicyclopentadiene acrylate, 4-chloromethylstyrene, acrylic acid, methyl acrylate, methacrylic acid, methyl methacrylate, glycidyl methacrylate, glycidyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, divinylbenzene and tripropylene glycol diacrylate.