Polyester polyol and method for producing same

By depolymerizing, esterifying and reducing compression polycondensation methods on the recycling of PET bottles, the problems of low-temperature torsional resistance and wear resistance of polyester polyol are solved, and the performance of polyester polyol is improved. The average molecular weight, acid value, glass transfer temperature and hydroxyl value achieve the optimization effect.

CN119019664APending Publication Date: 2024-11-26NANYA PLASTICS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310622333.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2023-05-30
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, polyester polyol made of recycling PET bottles has problems of low temperature torsion resistance and wear resistance.

Method used

A polyester polyol is used to produce a polyester polyol, including a depolymerization step to depolymerize the recovered PET bottle sheet, followed by an esterification reaction with polyether diol and dibasic acid, and finally obtain the polyester polyol by reducing the compression step. , control its number average molecular weight, acid value, glass transfer temperature and hydroxyl value to improve its performance.

Benefits of technology

Through this method, the low-temperature torsional and wear resistance of the polyester polyol is improved, with a number average molecular weight between 4,000 and 5,000, an acid price below 0.5 mgKOH/g, and a glass transfer temperature between -53°C and -50°C The hydroxyl value is between 40mmKOH/g and 50mmKOH/g, meeting the performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019664A_ABST
    Figure CN119019664A_ABST
Patent Text Reader

Abstract

The invention discloses polyester polyol and a preparation method thereof. The manufacturing method of the polyester polyol comprises a depolymerization step, an esterification step and a decompression polymerization step. In the depolymerization step, a plurality of recycled PET bottle flakes are depolymerized by a depolymerization solution to obtain a degradation product. The amount of the recycled PET flakes is between 20 parts by weight and 30 parts by weight, and the amount of the depolymerization liquid is between 28 parts by weight and 35 parts by weight. In the esterification step, the degradation product reacts with polyether glycol and dibasic acid to obtain a prepolymer. The amount of the polyether glycol is between 5 parts by weight and 10 parts by weight, and the amount of the binary acid is between 34 parts by weight and 40 parts by weight. In the step of decompression polymerization, the environmental pressure of the prepolymer is continuously reduced until the hydroxyl value of the prepolymer is less than 50mmKOH / g to obtain the polyester polyol, so that the problems of low-temperature bending resistance and poor wear resistance of the polyester polyol prepared from the recycled PET bottle chips in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polyester polyol and a preparation method thereof, in particular to a polyester polyol containing recycled PET bottle flakes and a preparation method thereof. Background Art

[0002] In the prior art, polyester polyols made from recycled PET bottle flakes have the problem of poor low-temperature bending resistance and abrasion resistance. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a polyester polyol and a method for preparing the same in view of the deficiencies in the prior art, so as to improve the problem in the prior art that the polyester polyol made from recycled PET bottle flakes has poor low-temperature bending resistance and wear resistance.

[0004] In order to solve the above technical problems, one of the technical solutions adopted by the present invention is to provide a method for producing polyester polyol, which comprises: a depolymerization step, depolymerizing a plurality of recycled PET bottle flakes with a depolymerization liquid to obtain a degradation product; wherein the amount of the recycled PET bottle flakes is between 20 parts by weight and 30 parts by weight, and the amount of the depolymerization liquid is between 28 parts by weight and 35 parts by weight; an esterification step, reacting the degradation product with a polyether diol and a dibasic acid to obtain a prepolymer; wherein the amount of the polyether diol is between 5 parts by weight and 10 parts by weight, and the amount of the dibasic acid is between 34 parts by weight and 40 parts by weight; and a reduced pressure polymerization step, continuously reducing the environmental pressure of the prepolymer until the hydroxyl value of the prepolymer is less than 50 mmKOH / g, to obtain a polyester polyol.

[0005] Preferably, the number average molecular weight of the polyester polyol is between 4,000 and 5,000.

[0006] Preferably, the depolymerization liquid is at least one selected from the group consisting of ethylene glycol, 1,4-butanediol and 1,6-hexanediol.

[0007] Preferably, the polyether diol is polytetramethylene ether, and the dibasic acid is at least one selected from the group consisting of adipic acid (AA), sebacic acid (SA), terephthalic acid (PTA) and isophthalic acid (IPA).

[0008] Preferably, the polyester polyol has an acid value of less than 0.5 mgKOH / g, a glass transition temperature between -53°C and -50°C, and a hydroxyl value between 40 mmKOH / g and 50 mmKOH / g.

[0009] In order to solve the above technical problems, another technical solution adopted by the present invention is to provide a polyester polyol, which is formed by reacting a plurality of recycled PET bottle flakes, a depolymerization liquid, a polyether diol and a dibasic acid; wherein the amount of the recycled PET bottle flakes is between 20 parts by weight and 30 parts by weight, the amount of the depolymerization liquid is between 28 parts by weight and 35 parts by weight, the amount of the polyether diol is between 5 parts by weight and 10 parts by weight, and the amount of the dibasic acid is between 34 parts by weight and 40 parts by weight; wherein the monohydroxy value of the polyester polyol is less than 50 mmKOH / g.

[0010] Preferably, the number average molecular weight of the polyester polyol is between 4,000 and 5,000.

[0011] Preferably, the depolymerization liquid is at least one selected from the group consisting of ethylene glycol, 1,4-butanediol and 1,6-hexanediol.

[0012] Preferably, the polyether diol is polytetramethylene ether, and the dibasic acid is at least one selected from the group consisting of adipic acid (AA), sebacic acid (SA), terephthalic acid (PTA) and isophthalic acid (IPA).

[0013] Preferably, the polyester polyol has an acid value of less than 0.5 mgKOH / g, a glass transition temperature between -53°C and -50°C, and a hydroxyl value between 40 mmKOH / g and 50 mmKOH / g.

[0014] One of the beneficial effects of the present invention is that the polyester polyol and the preparation method thereof provided by the present invention can improve the problem of poor low-temperature flexural resistance and wear resistance of the polyester polyol made from recycled PET bottle flakes in the prior art through the technical scheme of "the polyester polyol is formed by the reaction of the recycled PET bottle flakes, the depolymerization liquid, the polyether diol and the dibasic acid" and "the amount of the recycled PET bottle flakes is between 20 parts by weight and 30 parts by weight, the amount of the depolymerization liquid is between 28 parts by weight and 35 parts by weight, the amount of the polyether diol is between 5 parts by weight and 10 parts by weight, and the amount of the dibasic acid is between 34 parts by weight and 40 parts by weight".

[0015] To further understand the features and technical contents of the present invention, please refer to the following detailed description and drawings of the present invention. However, such description and drawings are only used to illustrate the present invention and are not intended to limit the protection scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The figure is a schematic flow chart of a method for producing polyester polyol according to an embodiment of the present invention. DETAILED DESCRIPTION

[0017] The following is an explanation of the implementation methods of the "polyester polyol and its production method" disclosed in the present invention through specific embodiments. Those skilled in the art can understand the advantages and effects of the present invention from the contents disclosed in this specification. The present invention can be implemented or applied through other different specific embodiments, and the details in this specification can also be modified and changed in various ways based on different viewpoints and applications without departing from the concept of the present invention. In addition, the drawings of the present invention are only simple schematic illustrations and are not depicted according to actual dimensions. It is stated in advance. The following embodiments will further explain the relevant technical contents of the present invention in detail, but the disclosed contents are not intended to limit the scope of protection of the present invention.

[0018] It should be understood that, although the terms "first", "second", "third", etc. may be used herein to describe various components or signals, these components or signals should not be limited by these terms. These terms are mainly used to distinguish one component from another component, or one signal from another signal. In addition, the term "or" used herein may include any one or more combinations of the associated listed items depending on the actual situation.

[0019] [Method for producing polyester polyol]

[0020] See also Figure 1 As shown, Figure 1 Schematic diagram of the process of manufacturing polyester polyols according to an embodiment of the present invention. The embodiment of the present invention provides a method for manufacturing polyester polyols, in particular, a method for manufacturing polyester polyols using recycled PET bottles. The method for manufacturing polyester polyols comprises a depolymerization step S110, an esterification step S120, and a reduced pressure polymerization step S130. Of course, the method for manufacturing polyester polyols may include other steps according to actual application requirements, but the present invention is not limited thereto.

[0021] In the depolymerization step S110, a plurality of recycled PET bottle flakes are depolymerized with a depolymerization liquid to obtain a degradation product. Specifically, in the depolymerization step S110, the recycled PET bottle flakes are mixed with the depolymerization liquid and a small amount of catalyst (such as zinc acetate), nitrogen is introduced, and the mixture is continuously stirred and gradually heated to between 200° C. and 230° C. (preferably about 215° C.) to obtain the transparent depolymerized product.

[0022] In the depolymerization step S110, the amount of the recycled PET bottle flakes is between 20 parts by weight and 30 parts by weight, and the amount of the depolymerization liquid is between 28 parts by weight and 35 parts by weight. It is worth mentioning that the depolymerization step S110 in the present invention is specifically for recycled PET bottle flakes, and the depolymerization step using mainly virgin polyester resin for depolymerization is not suitable for the depolymerization step S110 in the present invention.

[0023] In the depolymerization step S110 of this embodiment, the depolymerization liquid is at least one selected from the group consisting of ethylene glycol, 1,4-butanediol and 1,6-hexanediol. It is worth mentioning that since the chain length of ethylene glycol is shorter, when ethylene glycol is selected as the depolymerization liquid, the flexibility of the polyester polyol is less than ideal. Accordingly, the depolymerization liquid can exclude ethylene glycol and be limited to 1,4-butanediol or 1,6-hexanediol. Preferably, the depolymerization liquid is 1,4-butanediol.

[0024] In the esterification step S120, the degradation product is reacted with a polyether diol and a dibasic acid to obtain a prepolymer. Specifically, in the esterification step S120, after the degradation product is cooled to between 130°C and 160°C (preferably about 145°C), the polyether diol and the dibasic acid are added and the temperature is raised to between 175°C and 205°C (preferably about 190°C) for reaction for 1 hour, and then the temperature is further raised to between 200°C and 230°C (preferably about 215°C) for reaction for 2 hours, and then the water generated by the reaction is removed to form the prepolymer.

[0025] The amount of the polyether diol is between 5 parts by weight and 10 parts by weight, and the amount of the dibasic acid is between 34 parts by weight and 40 parts by weight. In the esterification step S120 of this embodiment, the polyether diol is polytetramethylene ether (PTMG), and the dibasic acid is at least one selected from the group of materials consisting of adipic acid (AA), sebacic acid (SA), terephthalic acid (PTA) and isophthalic acid (IPA). Preferably, the number average molecular weight of the polyether diol is between 1,000 and 2,000, and the dibasic acid is adipic acid.

[0026] In the reduced pressure polymerization step S130, the ambient pressure of the prepolymer is continuously reduced until the hydroxyl value of the prepolymer is less than 50 mmKOH / g to obtain a polyester polyol. Preferably, the polyester polyol has an acid value of less than 0.5 mgKOH / g, a glass transition temperature (Tg) between -53°C and -50°C, and a hydroxyl value between 40 mmKOH / g and 50 mmKOH / g, and the number average molecular weight of the polyester polyol is between 4,000 and 5,000. It is worth mentioning that in the reduced pressure polymerization step S130, the hydroxyl value of the prepolymer is controlled so that the polyester polyol can have a specific number average molecular weight.

[0027] [Polyester polyol]

[0028] This embodiment also provides a polyester polyol, which can be prepared by the aforementioned method for preparing polyester polyol, but the present invention is not limited thereto.

[0029] The polyester polyol is formed by reacting a plurality of recycled PET bottle flakes, a depolymerization liquid, a polyether diol and a dibasic acid. In terms of dosage, the amount of the recycled PET bottle flakes is between 20 parts by weight and 30 parts by weight, the amount of the depolymerization liquid is between 28 parts by weight and 35 parts by weight, the amount of the polyether diol is between 5 parts by weight and 10 parts by weight, and the amount of the dibasic acid is between 34 parts by weight and 40 parts by weight.

[0030] The depolymerization liquid is at least one selected from the group consisting of ethylene glycol, 1,4-butanediol and 1,6-hexanediol. Preferably, the depolymerization liquid is 1,4-butanediol or 1,6-hexanediol.

[0031] The polyether diol is polytetramethylene ether, and the dibasic acid is at least one selected from a group consisting of adipic acid (AA), sebacic acid (SA), terephthalic acid (PTA) and isophthalic acid (IPA). Preferably, the dibasic acid is adipic acid.

[0032] The polyester polyol has a number average molecular weight between 4,000 and 5,000, an acid value of less than 0.5 mgKOH / g, a glass transition temperature between -53°C and -50°C, and a hydroxyl value between 40 mmKOH / g and 50 mmKOH / g.

[0033] [Experimental data test]

[0034] Hereinafter, the present invention will be described in detail with reference to Examples 1 to 4 and Comparative Examples 1 to 3. However, the following examples are only used to help understand the present invention, and the scope of the present invention is not limited to these examples.

[0035] In Example 1, the polyester polyol is formed by reacting recycled PET bottle flakes, 1,4-butanediol (1,4-BG), polytetramethylene glycol (PTMG) and adipic acid (AA), the amount of recycled PET bottle flakes is 20.4 parts by weight, the amount of 1,4-butanediol is 34.8 parts by weight, the amount of polytetramethylene glycol is 5.3 parts by weight, and the amount of adipic acid is 49.5 parts by weight. The polytetramethylene glycol has a number average molecular weight of 1,000, and the polyester polyol has a number average molecular weight of 4,652, qualified low temperature bending resistance, a weight loss of 0.15% in abrasion resistance test, an acid value of 0.45 mgKOH / g, a glass transition temperature of -50.5°C, and a hydroxyl value of 42.3 mgKOH / g.

[0036] In Example 2, the polyester polyol is formed by reacting recycled PET bottle flakes, 1,4-butanediol (1,4-BG), polytetramethylene glycol (PTMG) and adipic acid (AA), the amount of recycled PET bottle flakes is 24.3 parts by weight, the amount of 1,4-butanediol is 32.1 parts by weight, the amount of polytetramethylene glycol is 6.2 parts by weight, and the amount of adipic acid is 37.4 parts by weight. The polytetramethylene glycol has a number average molecular weight of 1,000, and the polyester polyol has a number average molecular weight of 4,396, qualified low temperature bending resistance, a weight loss of 0.14% in abrasion resistance test, an acid value of 0.43 mgKOH / g, a glass transition temperature of -51.6°C, and a hydroxyl value of 46.1 mgKOH / g.

[0037] In Example 3, the polyester polyol is formed by reacting recycled PET bottle flakes, 1,4-butanediol (1,4-BG), polytetramethylene glycol (PTMG) and adipic acid (AA), the amount of recycled PET bottle flakes is 26.3 parts by weight, the amount of 1,4-butanediol is 30 parts by weight, the amount of polytetramethylene glycol is 8.5 parts by weight, and the amount of adipic acid is 35.2 parts by weight. The polytetramethylene glycol has a number average molecular weight of 1,000, and the polyester polyol has a number average molecular weight of 4,299, qualified low temperature bending resistance, a weight loss of 0.15% in abrasion resistance test, an acid value of 0.42 mgKOH / g, a glass transition temperature of -52.3°C, and a hydroxyl value of 45.6 mgKOH / g.

[0038] In Example 4, the polyester polyol is formed by reacting recycled PET bottle flakes, 1,4-butanediol (1,4-BG), polytetramethylene glycol (PTMG) and adipic acid (AA), the amount of recycled PET bottle flakes is 30 parts by weight, the amount of 1,4-butanediol is 28.2 parts by weight, the amount of polytetramethylene glycol is 9.8 parts by weight, and the amount of adipic acid is 32 parts by weight. The polytetramethylene glycol has a number average molecular weight of 1,000, and the polyester polyol has a number average molecular weight of 4,183, qualified low temperature bending resistance, a weight loss of 0.15% in abrasion resistance test, an acid value of 0.44 mgKOH / g, a glass transition temperature of -52.8°C, and a hydroxyl value of 48.3 mgKOH / g.

[0039] In Comparative Example 1, the polyester polyol is formed by reacting recycled PET bottle flakes, ethylene glycol (EG) and adipic acid (AA), the amount of recycled PET bottle flakes is 20.4 parts by weight, the amount of ethylene glycol is 30.3 parts by weight, and the amount of adipic acid is 59.7 parts by weight. The polyester polyol has a number average molecular weight of 4,112, unqualified low temperature bending resistance, a weight loss of 0.12% in abrasion resistance test, an acid value of 0.53 mgKOH / g, a glass transition temperature of -47.8°C, and a hydroxyl value of 48.8 mgKOH / g.

[0040] In Comparative Example 2, the polyester polyol is formed by reacting recycled PET bottle flakes, 1,4-butanediol (1,4-BG) and adipic acid (AA), the amount of recycled PET bottle flakes is 20.4 parts by weight, the amount of 1,4-butanediol is 37.2 parts by weight, and the amount of adipic acid is 42.2 parts by weight. The polyester polyol has a number average molecular weight of 4,200, unqualified low temperature bending resistance, a weight loss of 0.14% in abrasion resistance test, an acid value of 0.51 mgKOH / g, a glass transition temperature of -48.3°C, and a hydroxyl value of 45.8 mgKOH / g.

[0041] In Comparative Example 3, the polyester polyol is formed by reacting recycled PET bottle flakes, 1,4-butanediol (1,4-BG), polytetramethylene glycol (PTMG) and adipic acid (AA), the amount of recycled PET bottle flakes is 30 parts by weight, the amount of 1,4-butanediol is 27.5 parts by weight, the amount of polytetramethylene glycol is 10.5 parts by weight, and the amount of adipic acid is 34 parts by weight. The polytetramethylene glycol has a number average molecular weight of 1,000, the polyester polyol has a number average molecular weight of 4,140, ​​qualified low temperature bending resistance, a weight loss of 0.32% in abrasion resistance test, an acid value of 0.48 mgKOH / g, a glass transition temperature of -55.2°C, and a hydroxyl value of 48.1 mgKOH / g.

[0042] The composition ratios, low temperature flex resistance, abrasion resistance, acid value, glass transition temperature, and hydroxyl value of the polyester polyols of Examples 1 to 4 and Comparative Examples 1 to 3 are summarized in Table 1, and the related test methods are described below.

[0043] Low-temperature bending resistance: The test sample (4.5cm*7cm) was installed in a bending resistance tester (model GT-7006-V50). After 100,000 bending tests at an angle of 22.5°, a frequency of 100 times / minute and a temperature of -20°C, the surface of the test piece was observed to see if there was any damage (wrinkles and cracks).

[0044] Wear resistance: The test sample (outer diameter 10 cm, inner diameter 8 mm) was placed in an abrasion tester (model ABRASER-5130) with a grinding wheel model H-22, a weight of 1 kg and 1000 rotations. After the test, the weight loss percentage was calculated.

[0045] Acid value: Take 10 g of the sample (weigh accurately to four decimal places) in a conical flask, add 40 ml of ethanol and toluene (1:1) solution to dissolve, then add 3 drops of 0.1% phenolphthalein indicator, stir evenly, and titrate with 0.1N potassium hydroxide (KOH) aqueous solution until it turns slightly red (for ten seconds), and calculate the acid value according to the acid value formula.

[0046]

[0047] A is the titration amount of 0.1N KOH aqueous solution (ml)

[0048] N is the concentration of 0.1N KOH aqueous solution

[0049] S is the sample weight in g

[0050] Glass transition temperature: 5 mg of the sample was placed on a differential scanning calorimeter (model: TADSC25) and analyzed at a temperature of -90°C to 150°C at a rate of 20°C / min.

[0051] Hydroxyl value: Take 3g of sample from a round-bottom flask (weigh accurately to four decimal places), add 5ml of acetylation reagent (add 25ml of anhydrous acetic anhydride to 75ml of pyridine, mix well and set aside), heat to 95-100℃ for reaction for 1 hour, stop the reaction, add 1ml of distilled water, continue to heat to 95-100℃ for reaction for 1 hour, cool to room temperature, add 3 drops of 0.1% phenolphthalein indicator, titrate with 0.5N potassium hydroxide (KOH) aqueous solution until it turns slightly red (lasting for ten seconds), and calculate the hydroxyl value according to the hydroxyl value formula.

[0052]

[0053] A is the weight of the acetylated reagent in the blank test (g)

[0054] B is the weight of the acetylated reagent in the sample test (g)

[0055] C is the titration amount of 0.5N KOH aqueous solution in blank test (ml)

[0056] D is the titration amount of 0.5N KOH aqueous solution during the sample test (ml)

[0057] N is the concentration of 0.5N KOH aqueous solution

[0058] S is the sample weight in g

[0059] [Table 1: Ratio of ingredients and physicochemical properties of the examples and comparative examples]

[0060]

[0061] [Test results discussion]

[0062] As can be seen from Examples 1 to 4, the polyester polyol is formed by reacting 20.4 to 30 parts by weight of recycled PET bottle flakes, 28.2 to 34.8 parts by weight of depolymerization liquid, 5.3 to 9.8 parts by weight of polyether diol and 32 to 49.5 parts by weight of dibasic acid, and the polyester polyol has a number average molecular weight between 4183 and 4652, qualified low-temperature bending resistance, a weight loss between 0.14% and 0.15%, an acid value between 0.42 mmKOH / g and 0.45 mmKOH / g, a glass transition temperature between -52.8°C and -50.5°C, and a hydroxyl value between 42.3 mmKOH / g and 48.3 mmKOH / g.

[0063] It can be seen from Comparative Examples 1 and 2 that the polyester polyol does not contain polyether diol, resulting in the polyester polyol having unqualified low-temperature bending resistance, high acid value and high glass transition temperature.

[0064] It can be seen from Comparative Example 3 that using an excessive amount of polyether diol will result in a higher weight loss in the wear resistance test.

[0065] One of the beneficial effects of the present invention is that the polyester polyol and the preparation method thereof provided by the present invention can improve the problem of poor low-temperature flexural resistance and wear resistance of the polyester polyol made from recycled PET bottle flakes in the prior art through the technical scheme of "the polyester polyol is formed by the reaction of the recycled PET bottle flakes, the depolymerization liquid, the polyether diol and the dibasic acid" and "the amount of the recycled PET bottle flakes is between 20 parts by weight and 30 parts by weight, the amount of the depolymerization liquid is between 28 parts by weight and 35 parts by weight, the amount of the polyether diol is between 5 parts by weight and 10 parts by weight, and the amount of the dibasic acid is between 34 parts by weight and 40 parts by weight".

[0066] The contents disclosed above are only preferred feasible embodiments of the present invention, and are not intended to limit the scope of the present invention. Therefore, all equivalent technical changes made using the contents of the present invention's specification and drawings are included in the scope of the present invention.

Claims

1. A method for producing a polyester polyol, It is characterized in that The method for producing polyester polyol comprises: a depolymerization step, in which a plurality of recycled PET bottle flakes are depolymerized with a depolymerization liquid to obtain a degradation product; wherein the amount of the recycled PET bottle flakes is between 20 parts by weight and 30 parts by weight, and the amount of the depolymerization liquid is between 28 parts by weight and 35 parts by weight; an esterification step, reacting the degradation product with a polyether diol and a dibasic acid to obtain a prepolymer; wherein the amount of the polyether diol is between 5 parts by weight and 10 parts by weight, and the amount of the dibasic acid is between 34 parts by weight and 40 parts by weight; and A reduced pressure polymerization step is to continuously reduce the ambient pressure of the prepolymer until the hydroxyl value of the prepolymer is less than 50 mmKOH / g to obtain a polyester polyol.

2. The method for producing a polyester polyol according to claim 1, It is characterized in that The number average molecular weight of the polyester polyol is between 4,000 and 5,000.

3. The method for producing a polyester polyol according to claim 1, It is characterized in that The depolymerization liquid is at least one selected from the group consisting of ethylene glycol, 1,4-butanediol and 1,6-hexanediol.

4. The method for producing a polyester polyol according to claim 1, It is characterized in that The polyether diol is polytetramethylene ether, and the dibasic acid is at least one selected from a material group consisting of adipic acid, sebacic acid, terephthalic acid and isophthalic acid.

5. The method for producing a polyester polyol according to claim 1, It is characterized in that The polyester polyol has an acid value of less than 0.5 mgKOH / g, a glass transition temperature between -53°C and -50°C, and a hydroxyl value between 40 mmKOH / g and 50 mmKOH / g.

6. A polyester polyol, It is characterized in that The polyester polyol is formed by reacting a plurality of recycled PET bottle flakes, a depolymerization liquid, a polyether diol and a dibasic acid; The amount of the recycled PET bottle flakes is between 20 parts by weight and 30 parts by weight, the amount of the depolymerization liquid is between 28 parts by weight and 35 parts by weight, the amount of the polyether diol is between 5 parts by weight and 10 parts by weight, and the amount of the dibasic acid is between 34 parts by weight and 40 parts by weight; Wherein, the monohydroxy value of the polyester polyol is less than 50 mmKOH / g.

7. The polyester polyol according to claim 6, It is characterized in that The number average molecular weight of the polyester polyol is between 4,000 and 5,000.

8. The polyester polyol according to claim 6, It is characterized in that The depolymerization liquid is at least one selected from the group consisting of ethylene glycol, 1,4-butanediol and 1,6-hexanediol.

9. The polyester polyol according to claim 6, It is characterized in that The polyether diol is polytetramethylene ether, and the dibasic acid is at least one selected from a material group consisting of adipic acid, sebacic acid, terephthalic acid and isophthalic acid.

10. The polyester polyol according to claim 6, It is characterized in that The polyester polyol has an acid value of less than 0.5 mgKOH / g, a glass transition temperature between -53°C and -50°C, and a hydroxyl value between 40 mmKOH / g and 50 mmKOH / g.