High-toughness plastic packing material and preparation process thereof
By using materials such as polybutylene succinate PBS and specific preparation processes, a high-toughness plastic packaging material is formed, which solves the problem of insufficient toughness of existing foamed plastics, achieves high toughness and degradability, and meets the essence Application demands of cutting-edge industries.
Patent Information
- Application Number
- CN202411235282.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-26
AI Technical Summary
The existing foamed plastics have poor toughness and cannot meet the application needs of more sophisticated and cutting-edge industries.
Using polybutylene succinate PBS, castor oil modified hyperbranched polyurethane, modified glass fiber, peanut meal, jute fiber and other materials, through specific preparation processes and combination formulas, a high-toughness plastic packaging material is formed, with excellent Its fatigue resistance, heat resistance, weather resistance and corrosion resistance are completely decomposed in soil and water environments.
The preparation of high-toughness plastic packaging materials has been achieved, with excellent fatigue resistance and excellent heat, weather resistance and corrosion resistance. At the same time, the main material is a degradable plastic, which can be completely decomposed in the environment, extending the service life and improving the Oxidation resistance and mechanical properties.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of plastic packaging materials, and more specifically, to a high-toughness plastic packaging material and a preparation process thereof. Background Art
[0002] Plastic packaging refers to packaging made of plastic. Plastic is a type of material that uses synthetic or natural polymer resins as its main material. After adding various additives, it has ductility under certain temperature and pressure, and can fix its shape after cooling.
[0003] Foamed plastic is a new type of plastic material made by adding a foaming agent to create pores inside the plastic during the plastic production process. Almost all thermosetting and thermoplastic plastics can be made into foamed plastics, and commonly used resins include polystyrene, polyurethane, polyvinyl chloride, polyethylene, urea formaldehyde, phenolic formaldehyde, etc.
[0004] At present, foam plastics have been widely used in automobiles, home appliances, ships, air conditioners and mechanical products due to their good performance. However, the existing foam plastic products have poor toughness and cannot meet the application of more sophisticated industries.
[0005] Therefore, a solution needs to be proposed to solve this problem. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a high-toughness plastic packaging material and a preparation process thereof. The present invention has excellent anti-fatigue performance and excellent heat resistance, weather resistance and corrosion resistance, and the main materials are all degradable plastics, which can be completely decomposed into CO2 and H2O in soil and water environments.
[0007] The above technical purpose of the present invention is achieved through the following technical scheme: a high-toughness plastic packaging material, the raw materials of which include, by weight: 45-50 parts of polybutylene succinate PBS, 13-28 parts of castor oil modified hyperbranched polyurethane, 8-13 parts of modified glass fiber, 2.5-3 parts of peanut meal, 2-5 parts of jute fiber, 1.2-1.7 parts of titanate coupling agent, 2-3 parts of potassium sorbate, 1.1-1.6 parts of dehydroacetic acid, 14-18 parts of foaming agent, 5-8 parts of sodium citrate, 15-19 parts of ammonium bicarbonate, 2.7-2.9 parts of dimethyl phthalate, 2-5 parts of petroleum phenyl sulfonate, 3-5 parts of heavy calcium carbonate, 15-18 parts of quartz powder, 7-11 parts of kaolin, 5-9 parts of mica powder, 3-6 parts of decabromodiphenylethane, 2-4 parts of antimony trioxide, 2-4 parts of melamine, 1.2-1.8 parts of antioxidant, and 1.5-2.4 parts of antioxidant.
[0008] The present invention is further configured as follows: calculated by weight, the castor oil-modified hyperbranched polyurethane is prepared from the following components: 0.3 to 0.7 parts of small molecule polyol, 5.5 to 11.7 parts of dihydroxy acid, 24.3 to 36.5 parts of diisocyanate, 31.0 to 55.0 parts of macromolecular diol, 14.0 to 21.5 parts of ricinoleic acid and 1.0 to 3.7 parts of hydroxy acrylate.
[0009] The present invention is further configured as follows: the preparation steps of the modified glass fiber are as follows: a. Pretreatment: After preheating the glass fiber, firstly vacuum freeze-dry it, then mix it with hydrogen peroxide, heat it to 110-120°C, reflux for 1-2h, then add silane coupling agent, heat it to 90-100°C, continue to react for 3-6h, and after filtering and drying, the pre-modified glass fiber can be obtained;
[0010] b. Modification treatment: Pre-modified glass fiber and modified sol are heated at 90-120°C in a weight ratio of 1:(2-5) under vacuum conditions for 2-3 hours to obtain modified glass fiber.
[0011] The present invention is further configured as follows: the modified sol is composed of a mixed resin, a modified filler and a surfactant.
[0012] The present invention is further configured as follows: the mixed resin consists of carboxyl-terminated hyperbranched polyester, N,N-dimethylformamide and epoxy resin.
[0013] The present invention is further configured as follows: the protein content in the peanut meal is 40-47wt%.
[0014] The above technical purpose of the present invention is also achieved by the following technical scheme: A preparation process of a high-toughness plastic packaging material, comprising the following steps: Step S1: adding a titanate coupling agent to decabromodiphenylethane, antimony trioxide, melamine, heavy calcium carbonate, quartz powder, kaolin and mica powder, stirring at a stirring speed of 55 to 59 rpm for 7 to 11 minutes to obtain a modified filler;
[0015] Step S2: stirring the modified filler and 700-800 mesh peanut meal and jute fiber at a stirring speed of 70-74 rpm for 5-8 minutes, then adding castor oil modified hyperbranched polyurethane, modified glass fiber and polybutylene succinate, raising the temperature to 155-165° C. and continuing to stir at a stirring speed of 60-64 rpm for 8-11 minutes, then adding potassium sorbate, dehydroacetic acid, dimethyl phthalate, petroleum sulfonate phenyl ester, antioxidant and antioxidant, stirring at a stirring speed of 53-58 rpm for 25-28 minutes, then adding a foaming agent, sodium citrate and ammonium bicarbonate, stirring at a stirring speed of 57-61 rpm for 9-13 minutes to obtain a mixed material;
[0016] Step S3: adding the mixed material into an injection molding machine for injection molding to obtain a high-toughness plastic, wherein the injection molding pressure is 0.6-0.8 kPa and the injection molding temperature is 153-156°C.
[0017] In summary, the present invention has the following beneficial effects:
[0018] 1. The present invention has excellent fatigue resistance and excellent heat resistance, weather resistance and corrosion resistance, and the main ingredients are all degradable plastics, which can be completely decomposed into CO2 and H2O in soil and water environments; the addition of antioxidant SP and antioxidant DFC-34, the combined effect of the two greatly improves the oxidation resistance of the present invention, and it does not harden, break, shrink or warp during long-term use, and does not affect the viscosity, thereby extending the service life of the present invention; the use of peanut meal and jute fiber greatly improves the tensile resistance and toughness of the present invention, and soybean meal contains rich protein, which, when combined with the main ingredient, lengthens the length of the molecules in the main ingredient, greatly improving the mechanical properties of the present invention such as tensile strength and elongation at break;
[0019] 2. Through the pretreatment of glass fiber, the surface of pre-modified glass fiber is endowed with excellent bonding force. Then, in the subsequent modification process with modified sol, the mixed resin and modified filler can be stably combined and coated on the surface of pre-modified glass fiber to form a modified adhesive layer. Through the characteristics of the material itself and the compounding effect, the modified glass fiber and plastic are endowed with the advantages of high toughness and high torque;
[0020] 3. The present invention synthesizes a castor oil-modified hyperbranched polyurethane with a hyperbranched polyurethane as a core and ricinoleic acid as a shell. The polymer has low viscosity and is suitable for a high melt index polypropylene system. The polyurethane chain segment can provide good flexibility, and the ricinoleic acid coated on the outside can fully exert the plasticizing and toughening effects, reduce the brittleness of the polypropylene system, and increase the impact strength. DETAILED DESCRIPTION
[0021] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with specific embodiments. It should be noted that the embodiments of the present application and the features therein may be combined with each other without conflict.
[0022] In the description of the present invention, it should be noted that the terms "upper", "lower", "inside", "outside", "top / bottom" and the like indicating directions or positional relationships are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.
[0023] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "set / connected", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0024] The present invention is described in detail below.
[0025] A high-toughness plastic packaging material, the raw materials of which include, by weight: 45-50 parts of polybutylene succinate PBS, 13-28 parts of castor oil modified hyperbranched polyurethane, 8-13 parts of modified glass fiber, 2.5-3 parts of peanut meal, 2-5 parts of jute fiber, 1.2-1.7 parts of titanate coupling agent, 2-3 parts of potassium sorbate, 1.1-1.6 parts of dehydroacetic acid, 14-18 parts of foaming agent, citric acid 5-8 parts of sodium, 15-19 parts of ammonium bicarbonate, 2.7-2.9 parts of dimethyl phthalate, 2-5 parts of petroleum phenyl sulfonate, 3-5 parts of heavy calcium carbonate, 15-18 parts of quartz powder, 7-11 parts of kaolin, 5-9 parts of mica powder, 3-6 parts of decabromodiphenylethane, 2-4 parts of antimony trioxide, 2-4 parts of melamine, 1.2-1.8 parts of antioxidant, and 1.5-2.4 parts of antioxidant.
[0026] The castor oil-modified hyperbranched polyurethane is prepared from the following components, calculated by weight: 0.3-0.7 parts of small molecule polyol, 5.5-11.7 parts of dihydroxy acid, 24.3-36.5 parts of diisocyanate, 31.0-55.0 parts of macromolecular diol, 14.0-21.5 parts of ricinoleic acid and 1.0-3.7 parts of hydroxy acrylate.
[0027] The preparation steps of modified glass fiber are as follows: a. Pretreatment: After preheating the glass fiber, first vacuum freeze-dry it, then mix it with hydrogen peroxide, heat it to 110-120°C, reflux for 1-2h, then add silane coupling agent, heat it to 90-100°C, continue to react for 3-6h, and after filtering and drying, the pre-modified glass fiber can be obtained;
[0028] b. Modification treatment: Pre-modified glass fiber and modified sol are heated at 90-120°C in a weight ratio of 1:(2-5) under vacuum conditions for 2-3 hours to obtain modified glass fiber.
[0029] The modified sol is composed of mixed resin, modified filler and surfactant, and the mixed resin is composed of terminal carboxyl hyperbranched polyester, N,N-dimethylformamide and epoxy resin.
[0030] The protein content in peanut meal is 40-47wt%.
[0031] A preparation process of a high-toughness plastic packaging material comprises the following steps: Step S1: adding a titanate coupling agent to decabromodiphenylethane, antimony trioxide, melamine, heavy calcium carbonate, quartz powder, kaolin and mica powder, and stirring at a stirring speed of 55 to 59 rpm for 7 to 11 minutes to obtain a modified filler;
[0032] Step S2: stirring the modified filler and 700-800 mesh peanut meal and jute fiber at a stirring speed of 70-74 rpm for 5-8 minutes, then adding castor oil modified hyperbranched polyurethane, modified glass fiber and polybutylene succinate, raising the temperature to 155-165° C. and continuing to stir at a stirring speed of 60-64 rpm for 8-11 minutes, then adding potassium sorbate, dehydroacetic acid, dimethyl phthalate, petroleum sulfonate phenyl ester, antioxidant and antioxidant, stirring at a stirring speed of 53-58 rpm for 25-28 minutes, then adding a foaming agent, sodium citrate and ammonium bicarbonate, stirring at a stirring speed of 57-61 rpm for 9-13 minutes to obtain a mixed material;
[0033] Step S3: adding the mixed material into an injection molding machine for injection molding to obtain a high-toughness plastic, wherein the injection molding pressure is 0.6-0.8 kPa and the injection molding temperature is 153-156°C.
[0034] The invention synthesizes a castor oil modified hyperbranched polyurethane with a hyperbranched polyurethane as a core and ricinoleic acid as a shell. The polymer has low viscosity and is suitable for a high melt index polypropylene system. The polyurethane chain segment can provide good flexibility, and the ricinoleic acid coated on the outside can fully exert the plasticizing and toughening effects, reduce the brittleness of the polypropylene system, and increase the impact strength. In addition, the polymer has a large molecular weight and is resistant to migration and precipitation compared with a modified vegetable oil plasticizer with a small molecular weight. Acrylic double bonds are introduced into the castor oil modified hyperbranched polyurethane, which can react with an acrylamide methyl substituted cellulose ester polymer in a cross-linking reaction during processing to form a network structure, thereby improving the tensile modulus, strength, and heat deformation temperature of the plastic system.
[0035] Through the pretreatment of glass fiber, the surface of pre-modified glass fiber is endowed with excellent bonding force. Then, in the subsequent modification process with modified sol, the mixed resin and modified filler can be stably combined and coated on the surface of pre-modified glass fiber to form a modified adhesive layer. Through the characteristics of the material itself and the compounding effect, the modified glass fiber and plastic are endowed with the advantages of high toughness and high torque. Through the mixed resin with a specific ratio, the modified adhesive layer is guaranteed to be fully grafted and cross-linked with the surface of the pre-modified glass fiber. While the synergistic effect of the three is good, the formed modified adhesive layer itself has strong anti-warping and toughness, which in turn ensures the high toughness and high torque of the modified glass fiber.
[0036] The invention adopts polybutylene succinate (PBS) as the main material, so that the invention has excellent fatigue resistance and excellent heat resistance, weather resistance and corrosion resistance, and the main materials are all degradable plastics, which can be completely decomposed into CO2 and H2O in soil and water environment; antioxidant SP and antioxidant DFC-34 are added, and the combined effect of the two greatly improves the oxidation resistance of the invention, and the invention does not harden, break, shrink or warp during long-term use, and does not affect the viscosity, thereby extending the service life of the invention; peanut meal and jute fiber are used in combination, which greatly improves the tensile resistance and toughness of the invention, and soybean meal contains rich protein, which is combined with the main material to lengthen the length of the molecules in the main material, greatly improving the mechanical properties of the invention such as tensile strength and elongation at break; heavy calcium carbonate, quartz powder, kaolin and mica powder are used as fillers The reinforcing agent is added to greatly improve the wear resistance of the invention, and through the effect of the titanate coupling agent NDZ-101, the inorganic raw materials and the main material form a whole, and the added dimethyl phthalate DMP and petroleum sulfonate phenyl ester M-50 are used as plasticizers to make the barite powder, pyroxene powder, white carbon black and mica powder evenly distributed in the main material, thereby ensuring the consistency of the performance of the invention; potassium sorbate and dehydroacetic acid are added as preservatives to effectively kill microorganisms, thereby extending the service life of the invention; foaming agent TSH, sodium citrate, and ammonium bicarbonate are used as foaming agents, and heating and decomposition generate gas to form pores, with a large gas emission and uniform foaming, which greatly improves the pressure resistance and tensile strength of the invention; the flame retardant system composed of decabromodiphenylethane, antimony trioxide and melamine can effectively improve the flame retardancy and heat resistance of the invention.
[0037] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A high-toughness plastic packaging material, the raw materials of which include by weight: 45-50 parts of polybutylene succinate PBS, 13-28 parts of castor oil modified hyperbranched polyurethane, 8-13 parts of modified glass fiber, 2.5-3 parts of peanut meal, 2-5 parts of jute fiber, 1.2-1.7 parts of titanate coupling agent, 2-3 parts of potassium sorbate, 1.1-1.6 parts of dehydroacetic acid, 14-18 parts of foaming agent, 5-8 parts of sodium citrate, 15-19 parts of ammonium bicarbonate, 2.7-2.9 parts of dimethyl phthalate, 2-5 parts of petroleum sulfonate phenyl ester, 3-5 parts of heavy calcium carbonate, 15-18 parts of quartz powder, 7-11 parts of kaolin, 5-9 parts of mica powder, 3-6 parts of decabromodiphenylethane, 2-4 parts of antimony trioxide, 2-4 parts of melamine, 1.2-1.8 parts of antioxidant, 1.5-2.4 parts of antioxidant.
2. A high-toughness plastic packaging material according to claim 1, characterized in that: The castor oil-modified hyperbranched polyurethane is prepared from the following components calculated by weight: 0.3-0.7 parts of small molecule polyol, 5.5-11.7 parts of dihydroxy acid, 24.3-36.5 parts of diisocyanate, 31.0-55.0 parts of macromolecular diol, 14.0-21.5 parts of ricinoleic acid and 1.0-3.7 parts of hydroxy acrylate.
3. The high-toughness plastic packaging material according to claim 1, characterized in that: The preparation steps of the modified glass fiber are as follows: a. Pretreatment: After preheating the glass fiber, first perform vacuum freeze drying on it, then mix it with hydrogen peroxide, heat it to 110-120°C, reflux for 1-2h, then add silane coupling agent, heat it to 90-100°C, continue to react for 3-6h, and after filtering and drying, the pre-modified glass fiber can be obtained; b. Modification treatment: Pre-modified glass fiber and modified sol are heated at 90-120°C in a weight ratio of 1:(2-5) under vacuum conditions for 2-3 hours to obtain modified glass fiber.
4. A high-toughness plastic packaging material and a preparation process thereof according to claim 3, characterized in that: The modified sol consists of mixed resin, modified filler and surfactant.
5. The high-toughness plastic packaging material according to claim 4, characterized in that: The mixed resin consists of carboxyl-terminated hyperbranched polyester, N,N-dimethylformamide and epoxy resin.
6. The high-toughness plastic packaging material according to claim 1, characterized in that: The protein content of the peanut meal is 40-47 wt%.
7. A process for preparing a high-toughness plastic packaging material according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: Step S1: adding a titanate coupling agent to decabromodiphenylethane, antimony trioxide, melamine, heavy calcium carbonate, quartz powder, kaolin and mica powder, stirring at a stirring speed of 55 to 59 rpm for 7 to 11 minutes to obtain a modified filler; Step S2: stirring the modified filler and 700-800 mesh peanut meal and jute fiber at a stirring speed of 70-74 rpm for 5-8 minutes, then adding castor oil modified hyperbranched polyurethane, modified glass fiber and polybutylene succinate, raising the temperature to 155-165° C. and continuing to stir at a stirring speed of 60-64 rpm for 8-11 minutes, then adding potassium sorbate, dehydroacetic acid, dimethyl phthalate, petroleum sulfonate phenyl ester, antioxidant and antioxidant, stirring at a stirring speed of 53-58 rpm for 25-28 minutes, then adding a foaming agent, sodium citrate and ammonium bicarbonate, stirring at a stirring speed of 57-61 rpm for 9-13 minutes to obtain a mixed material; Step S3: adding the mixed material into an injection molding machine for injection molding to obtain a high-toughness plastic, wherein the injection molding pressure is 0.6-0.8 kPa and the injection molding temperature is 153-156°C.