Inorganic protective coating for high-temperature and wear environments and preparation method of inorganic protective coating
Through the combination of inorganic protective coatings and high-temperature treatment technology, high-temperature, heat shock and wear-resistant coatings are formed, which solves the problem of insufficient protection in the existing technology in high temperature and wear environments, and significantly improves the metal substrate Lifespan and performance.
Patent Information
- Application Number
- CN202310597904.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is difficult to effectively protect metal substrates in high temperature and wear environments, resulting in a shortening of the service life of the gun barrel and flight armament, and the organic protective coating lacks high temperature resistance.
Using an inorganic protective coating, including matrix aluminum source, silicon source, oxide, thermal expansion adjustment and wear-resistant enhancement dual-function filler and compacting agent, the coating is enhanced by high-temperature treatment and sintering. Hardness, adhesion and thermal expansion matching, form an adhesive layer to improve high temperature resistance, heat shock resistance and wear resistance.
It achieves high performance protection under high temperatures above 800℃ and over 100 thermal shock cycles. The hardness, adhesion and wear resistance of the coating are significantly improved, the wear amount is less than 5mg, and the thermal expansion coefficient is adjustable, suitable for different metal bases. material.
Smart Images

Figure BDA0004247781640000061
Abstract
Description
Technical Field
[0001] The invention belongs to the field of high-temperature protection of metals, and in particular relates to an inorganic protective coating used in high-temperature and wear environments and a preparation method thereof. Background Art
[0002] When a shell is fired, on the one hand, the propellant burns in the inner bore of the barrel to produce high-temperature and high-pressure gas, causing ablation of the inner bore of the barrel; on the other hand, the shell will also cause mechanical wear to the inner bore during its operation in the barrel, causing ablation and wear of the inner bore of the barrel, seriously affecting the service life of the barrel. In addition, flying armaments such as rockets, missiles, and fighter planes will rub against the air when flying at high speed in the air, thereby generating high temperatures, causing wear and high-temperature damage to the surface of the flying armaments, affecting the safe flight of the flying armaments. All of the above show that how to protect metal substrates from high temperatures and wear in high temperature and wear environments has important military significance. Organic protective coatings are generally difficult to solve the problem of high temperature resistance, so the present invention is based on pure inorganic materials to develop an inorganic protective coating that is resistant to high temperatures, thermal shock, and wear. Summary of the invention
[0003] In order to overcome the deficiencies of the prior art, the present invention provides an inorganic protective coating that is resistant to high temperature, thermal shock and wear, and a preparation method thereof.
[0004] The solution adopted by the present invention to solve its technical problem is: an inorganic protective coating for high temperature and wear environment, the raw materials include the following components by weight: 20 to 30 parts of matrix aluminum source, 20 to 30 parts of matrix silicon source, 10 to 15 parts of matrix oxide, 15 to 30 parts of thermal expansion regulating and wear resistance enhancing dual-functional filler, and 10 to 20 parts of densifier.
[0005] Preferably, the matrix aluminum source is one, two or three of aluminum oxide, calcium aluminate and potassium aluminate.
[0006] Preferably, the matrix silicon source is one, two or three of silicon dioxide, sodium silicate and calcium silicate.
[0007] Preferably, the matrix oxide is one or a combination of two or more of sodium oxide, potassium oxide, lithium oxide, calcium oxide and magnesium oxide.
[0008] The matrix aluminum source, matrix silicon source and matrix oxide undergo complex physical and chemical changes including physical state transformation and ion exchange at high temperatures of 1400-1700°C in an air environment to form a matrix phase. The matrix phase is mainly a specific amorphous and a small amount of crystalline mixed structure composed of aluminates and silicates, which can withstand temperatures above 800°C.
[0009] Preferably, the dual-functional filler for thermal expansion regulation and wear resistance enhancement is one or a combination of two or more of silicon carbide, silicon nitride, boron nitride and mullite.
[0010] Preferably, the dual-functional filler for thermal expansion regulation and wear resistance enhancement is a granular, flaky, whisker or fibrous material.
[0011] Silicon carbide, silicon nitride, boron nitride, and mullite have the following advantages as dual-functional fillers for thermal expansion regulation and wear resistance enhancement: (1) They have a high melting point and thermal stability, and are chemically inert in the coating, so that the coating remains unchanged after forming; (2) During the sintering process of the coating, they have good wettability to the molten matrix phase, thereby reducing the surface tension and achieving a close bond with the matrix phase; (3) They themselves have a high hardness and are not easily detached or consumed during wear, which can improve the overall wear resistance of the coating; (4) They themselves have a high strength and can be used for external toughening of the coating matrix, improving the overall toughness and strength of the coating through mechanisms such as pulling out and bridging; (5) They have a low thermal expansion coefficient, which can effectively reduce the overall thermal expansion coefficient of the coating to achieve matching with the thermal expansion coefficient of the metal substrate.
[0012] Preferably, the compacting agent is one or a combination of two or more of phosphorus pentoxide, boron oxide, bismuth oxide and iron oxide.
[0013] During the coating sintering process, phosphorus pentoxide, boron oxide, bismuth oxide, and iron oxide can reduce the softening point of the matrix phase and reduce the viscosity of the coating in the sintered state, which is conducive to the removal of gas inside the coating during the sintering process, obtaining a denser microstructure and improving the hardness of the coating. In addition, the densifier can also reduce the roughness of the coating surface, making the coating surface smoother, thereby reducing friction and further reducing the heat generated by friction.
[0014] The present invention also discloses a method for preparing an inorganic protective coating for high temperature and wear environment, comprising the following steps:
[0015] (1) taking 20 to 30 parts of a matrix aluminum source, 20 to 30 parts of a matrix silicon source, 10 to 15 parts of a matrix oxide, 15 to 30 parts of a dual-function filler for thermal expansion adjustment and wear resistance enhancement, and 10 to 20 parts of a densifier, and mixing them thoroughly to obtain powder A;
[0016] (2) heating powder A at a high temperature of 1400 to 1700° C. in an air atmosphere for 30 to 50 minutes, and quenching to obtain a block B;
[0017] (3) Grinding block B into powder to obtain powder C;
[0018] (4) using a dry method or a wet method to uniformly apply powder C to the surface of a metal substrate, and controlling the coating thickness to be 50 to 400 μm;
[0019] (5) The coated metal substrate is placed in a high temperature furnace preheated to 900-1100° C. for 15 minutes, then taken out and cooled in air.
[0020] Furthermore, after the coating is sintered and formed, a bonding layer is formed at the interface between the coating and the metal substrate.
[0021] In terms of chemical composition, the bonding layer is composed of coating elements and metal substrate elements, with the metal substrate elements gradually decreasing and the coating elements gradually increasing from the metal substrate to the coating. In terms of microscopic morphology, during the high-temperature sintering process, part of the room-temperature metallographic phase in the metal substrate transforms into the high-temperature metallographic phase, the interface becomes rough, and the coating and the metal substrate form a mutual bite, which significantly improves the adhesion between the coating and the metal substrate.
[0022] Furthermore, the matrix aluminum source is one or two or three of aluminum oxide, calcium aluminate, and potassium aluminate; the matrix silicon source is one or two or three of silicon dioxide, sodium silicate, and calcium silicate; the matrix oxide is one or a combination of two or more of sodium oxide, potassium oxide, lithium oxide, calcium oxide, and magnesium oxide; the thermal expansion regulating and wear-resistant enhancing dual-functional filler is one or a combination of two or more of silicon carbide, silicon nitride, boron nitride, and mullite; the compacting agent is one or a combination of two or more of phosphorus pentoxide, boron oxide, bismuth oxide, and iron oxide.
[0023] Furthermore, the porosity of the coating is below 3%.
[0024] Furthermore, the coating has a thickness of 50 to 400 μm.
[0025] Furthermore, the thermal expansion coefficient of the coating is 8×10 -6 / ℃~14×10 -6 / ℃ range is adjustable and can be applied to different metal substrates such as steel.
[0026] Furthermore, the hardness of the coating is 900-1300 HV.
[0027] Furthermore, the adhesion between the coating and the metal substrate is 10 to 15 MPa.
[0028] An inorganic protective coating for high temperature and wear environment as described above, the excellent wear resistance of the coating is achieved through the high adhesion between the coating and the metal substrate, the high hardness of the coating, and the smooth surface of the coating. First, the hardness of the substrate itself is high, the dual-functional filler of thermal expansion regulation and wear resistance enhancement can increase the hardness of the coating, and the densifier further increases the overall hardness of the coating by reducing the porosity, so that the coating itself is not easy to wear; secondly, the coating has high adhesion to the metal substrate, so that the coating is not easy to fall off from the metal substrate under wear conditions; finally, the densifier reduces the roughness of the coating surface, making the coating surface smoother, so that under the same external conditions, the friction of the coating surface is small, and the coating is less likely to be worn.
[0029] An inorganic protective coating for high temperature and wear environment as described above, the excellent thermal shock resistance of the coating is achieved by the high adhesion between the coating and the metal substrate and the good thermal expansion matching between the coating and the metal substrate. On the one hand, the thermal expansion matching between the coating and the metal substrate is good, the deformation of the coating and the metal substrate is consistent under thermal shock conditions, the residual stress inside the coating is small, and the coating is not easy to crack; on the other hand, the adhesion between the coating and the metal substrate is high, even if the coating cracks, the coating is not easy to fall off, so it still has high temperature protection ability.
[0030] In summary, the present invention, based on the selection of appropriate matrix phase materials and relative dosage, significantly improves the high temperature resistance, thermal shock resistance and wear resistance of the coating through the synergistic strengthening effect of thermal expansion adjustment and wear-resistant enhancement dual-functional fillers and densifiers on the thermal expansion coefficient, porosity, surface roughness, hardness and adhesion of the coating. The coating of the present invention has the following beneficial effects: (1) good high temperature resistance, which can withstand a high temperature of 800°C; (2) good thermal shock resistance, which can withstand more than 100 thermal shock cycles at 800°C; (3) good wear resistance, with a rubber grinding wheel wearing 3000 revolutions under a load of 1kg, and the wear mass is less than 5mg. DETAILED DESCRIPTION
[0031] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0032] Example 1
[0033] The preparation of Example 1 includes the following raw materials and processes:
[0034] (1) 50 g of aluminum oxide, 75 g of calcium aluminate, 25 g of potassium aluminate, 50 g of silicon dioxide, 50 g of potassium silicate, 25 g of sodium oxide, 25 g of potassium oxide, 75 g of silicon carbide, 75 g of boron nitride, 15 g of phosphorus pentoxide, 25 g of boron oxide, and 10 g of bismuth oxide were mixed thoroughly to obtain powder A;
[0035] (2) heating powder A at 1680°C in an air atmosphere for 30 minutes and quenching to obtain block B;
[0036] (3) Grinding block B into powder to obtain powder C;
[0037] (4) Powder C is evenly applied to the steel surface by dry method with a thickness of 375 μm;
[0038] (5) The coated steel substrate is placed in a high temperature furnace preheated to 1060° C. for 15 minutes, then taken out and cooled in air.
[0039] Example 2
[0040] The preparation of Example 2 includes the following raw materials and processes:
[0041] (1) 50 g of calcium aluminate, 75 g of potassium aluminate, 125 g of sodium silicate, 15 g of potassium oxide, 25 g of lithium oxide, 10 g of calcium oxide, 25 g of magnesium oxide, 75 g of silicon carbide, 75 g of bismuth oxide, and 25 g of iron oxide were mixed thoroughly to obtain powder A;
[0042] (2) heating powder A at 1400°C in an air atmosphere for 50 minutes and quenching to obtain block B;
[0043] (3) Grinding block B into powder to obtain powder C;
[0044] (4) Powder C is evenly applied to the steel surface by dry method with a thickness of 210 μm;
[0045] (5) The coated steel substrate is placed in a high-temperature furnace preheated to 900° C. for 15 minutes, then taken out and cooled in air.
[0046] Example 3
[0047] The preparation of Example 3 includes the following raw materials and processes:
[0048] (1) 100 g of calcium aluminate, 50 g of silicon dioxide, 50 g of sodium silicate, 50 g of potassium silicate, 20 g of sodium oxide, 15 g of lithium oxide, 25 g of calcium oxide, 25 g of silicon nitride, 25 g of boron nitride, 75 g of mullite, and 65 g of boron oxide were mixed thoroughly to obtain powder A;
[0049] (2) heating powder A at 1520°C in an air atmosphere for 40 minutes and quenching to obtain block B;
[0050] (3) Grinding block B into powder to obtain powder C;
[0051] (4) Powder C is evenly coated on the steel surface by wet method with a thickness of 55 μm;
[0052] (5) The coated steel substrate is placed in a high-temperature furnace preheated to 930° C. for 15 minutes, then taken out and cooled in air.
[0053] Comparative Example 1
[0054] The preparation of Comparative Example 1 includes the following raw materials and processes:
[0055] (1) 50 g of calcium aluminate, 75 g of potassium aluminate, 15 g of potassium oxide, 25 g of lithium oxide, 10 g of calcium oxide, 25 g of magnesium oxide, 75 g of silicon carbide, 75 g of bismuth oxide, and 25 g of iron oxide were mixed thoroughly to obtain powder A;
[0056] (2) heating powder A at 1400°C in an air atmosphere for 50 minutes and quenching to obtain block B;
[0057] (3) Grinding block B into powder to obtain powder C;
[0058] (4) Powder C is evenly applied to the steel surface by dry method with a thickness of 210 μm;
[0059] (5) The coated steel substrate is placed in a high-temperature furnace preheated to 900° C. for 15 minutes, then taken out and cooled in air.
[0060] Comparative Example 2
[0061] The preparation of Comparative Example 2 includes the following raw materials and processes:
[0062] (1) 50 g of calcium aluminate, 75 g of potassium aluminate, 125 g of sodium silicate, 15 g of potassium oxide, 25 g of lithium oxide, 10 g of calcium oxide, 25 g of magnesium oxide, 75 g of bismuth oxide, and 25 g of iron oxide were mixed thoroughly to obtain powder A;
[0063] (2) heating powder A at 1400°C in an air atmosphere for 50 minutes and quenching to obtain block B;
[0064] (3) Grinding block B into powder to obtain powder C;
[0065] (4) Powder C is evenly applied to the steel surface by dry method with a thickness of 210 μm;
[0066] (5) The coated steel substrate is placed in a high-temperature furnace preheated to 900° C. for 15 minutes, then taken out and cooled in air.
[0067] Comparative Example 3
[0068] The preparation of Comparative Example 3 includes the following raw materials and processes:
[0069] (1) 50 g of calcium aluminate, 75 g of potassium aluminate, 125 g of sodium silicate, 15 g of potassium oxide, 25 g of lithium oxide, 10 g of calcium oxide, 25 g of magnesium oxide, and 75 g of silicon carbide were mixed thoroughly to obtain powder A;
[0070] (2) heating powder A at 1400°C in an air atmosphere for 50 minutes and quenching to obtain block B;
[0071] (3) Grinding block B into powder to obtain powder C;
[0072] (4) Powder C is evenly applied to the steel surface by dry method with a thickness of 210 μm;
[0073] (5) The coated steel substrate is placed in a high-temperature furnace preheated to 900° C. for 15 minutes, then taken out and cooled in air.
[0074] In order to verify the implementation effect of the present invention, the following analysis and experiments were carried out.
[0075] Among them, since the comparative example 1 lacked silicon source in the matrix phase and the coating forming condition was poor, no other measurements and analyses were performed.
[0076] (1) Basic performance indicators of coatings
[0077] Table 1 shows the basic performance indicators of the coatings described in Examples 1-3 and Comparative Examples 2 and 3. It can be seen from Table 1 that Examples 1-3, Comparative Example 2 and Comparative Example 3 all have excellent high temperature resistance and can withstand temperatures above 800°C. Examples 1-3 all have extremely low porosity (<3%), smooth surface (Ra<0.35μm), microhardness between 900 and 1300HV, adhesion between 10 and 15MPa, thermal expansion coefficient between 8×10 -6 / ℃~14×10 -6 / ℃. Without adding any dual-functional fillers for thermal expansion regulation and wear-resistance enhancement (Comparative Example 2), the hardness of the coating is significantly reduced, and the thermal expansion coefficient is significantly larger, indicating that the dual-functional fillers for thermal expansion regulation and wear-resistance enhancement play an important role in the hardness and thermal expansion behavior of the coating. Without adding any densifier (Comparative Example 3), the porosity and surface roughness Ra of the coating are significantly larger, and the hardness is significantly reduced. In addition, the reduction in adhesion may be caused by the increase in porosity. It can be seen that the densifier has a significant effect on porosity, surface roughness, microhardness and adhesion.
[0078] Table 1 Basic properties of the coatings described in Examples 1-3 and Comparative Examples 2 and 3
[0079]
[0080] (2) Wear resistance
[0081] A rotating rubber grinding wheel wear tester was used, and the wear was performed for 3000 revolutions under a load of 1kg. The wear mass was weighed and calculated by an electronic scale, and the wear resistance of the coating was evaluated by the wear mass. The wear mass loss of Examples 1-3 and Comparative Examples 2 and 3 is shown in Table 2. It can be seen that Examples 1-3 all have excellent wear resistance, and their wear amount is not more than 5mg. In the absence of the addition of the dual-functional filler for thermal expansion adjustment and wear-resistant enhancement (Comparative Example 2), the wear amount of the coating increased to 59mg, which indicates that the dual-functional filler for thermal expansion adjustment and wear-resistant enhancement can increase the hardness of the coating and thus improve the wear resistance of the coating. In the absence of the addition of a densifier (Comparative Example 3), the wear mass of the coating deteriorated significantly (120mg), indicating that the densifier plays an important role in improving the wear resistance of the coating, because the densifier can increase the density, hardness and adhesion of the coating, and reduce the surface roughness of the coating.
[0082] Table 2 Wear quality of the coatings described in Examples 1-3 and Comparative Examples 2 and 3
[0083] Example 1 Example 2 Example 3 Comparative Example 2 Comparative Example 3 Wear / mg 2 5 3 59 120
[0084] (3) Thermal shock resistance
[0085] The muffle furnace was preheated to 800°C, and the coating specimen was placed in it and maintained for 5 minutes. The specimen was taken out and cooled to room temperature in the air for one cycle. The test was carried out 100 times in total, and the coating surface was observed for degradation such as shedding to evaluate the thermal shock resistance of the coating. The results show that Examples 1-3 can withstand more than 100 thermal shock cycles, while Comparative Example 2 and Comparative Example 3 deteriorated significantly after 8 and 58 thermal shock cycles, respectively, indicating that the thermal expansion regulating and wear-resistant enhancing dual-functional fillers and densifiers have a significant effect on the thermal shock resistance of the coating. Among them, the thermal expansion regulating and wear-resistant enhancing dual-functional fillers improve the thermal shock resistance of the coating by improving the thermal expansion matching between the coating and the technical substrate, and the densifier improves the thermal shock resistance of the coating by improving the adhesion.
Claims
1. An inorganic protective coating for high temperature and wear environment, characterized in that: The raw materials include the following components by weight: 20-30 parts of matrix aluminum source, 20-30 parts of matrix silicon source, 10-15 parts of matrix oxide, 15-30 parts of thermal expansion regulating and wear-resistant reinforcing dual-functional filler, and 10-20 parts of densifier.
2. The inorganic protective coating for high temperature and wear environment according to claim 1, characterized in that: The matrix aluminum source is one, two or three of aluminum oxide, calcium aluminate and potassium aluminate.
3. The inorganic protective coating for high temperature and wear environment according to claim 1, characterized in that: The matrix silicon source is one, two or three of silicon dioxide, sodium silicate and calcium silicate.
4. The inorganic protective coating for high temperature and wear environment according to claim 1, characterized in that: The matrix oxide is one or a combination of two or more of sodium oxide, potassium oxide, lithium oxide, calcium oxide and magnesium oxide.
5. The inorganic protective coating for high temperature and wear environment according to claim 1, characterized in that: The dual-function filler for thermal expansion adjustment and wear resistance enhancement is one or a combination of two or more of silicon carbide, silicon nitride, boron nitride and mullite.
6. The inorganic protective coating for high temperature and wear environment according to claim 1, characterized in that: The compacting agent is one or a combination of two or more of phosphorus pentoxide, boron oxide, bismuth oxide and iron oxide.
7. A method for preparing an inorganic protective coating for high temperature and wear environment, characterized by comprising the following steps: (1) taking 20 to 30 parts of a matrix aluminum source, 20 to 30 parts of a matrix silicon source, 10 to 15 parts of a matrix oxide, 15 to 30 parts of a dual-function filler for thermal expansion adjustment and wear resistance enhancement, and 10 to 20 parts of a densifier, and mixing them thoroughly to obtain powder A; (2) heating powder A at a high temperature of 1400 to 1700° C. in an air atmosphere for 30 to 50 minutes, and quenching to obtain a block B; (3) Grinding block B into powder to obtain powder C; (4) using a dry method or a wet method to uniformly apply powder C to the surface of a metal substrate, and controlling the coating thickness to be 50 to 400 μm; (5) The coated metal substrate is placed in a high temperature furnace preheated to 900-1100° C. for 15 minutes, then taken out and cooled in air.
8. The method for preparing an inorganic protective coating for high temperature and wear environment according to claim 7, characterized in that: After the coating is fired and formed, a bonding layer is formed at the interface between the coating and the metal substrate.
9. The method for preparing an inorganic protective coating for high temperature and wear environment according to claim 7, characterized in that: The matrix aluminum source is one or two or three of aluminum oxide, calcium aluminate, and potassium aluminate; the matrix silicon source is one or two or three of silicon dioxide, sodium silicate, and calcium silicate; the matrix oxide is one or a combination of two or more of sodium oxide, potassium oxide, lithium oxide, calcium oxide, and magnesium oxide; the thermal expansion regulating and wear-resistant enhancing dual-function filler is one or a combination of two or more of silicon carbide, silicon nitride, boron nitride, and mullite; the compacting agent is one or a combination of two or more of phosphorus pentoxide, boron oxide, bismuth oxide, and iron oxide.
10. The method for preparing an inorganic protective coating for high temperature and wear environment according to claim 7, characterized in that: The porosity of the coating is less than 3%, the hardness of the coating is 900-1300 HV, and the adhesion between the coating and the metal substrate is 10-15 MPa.
Citation Information
Patent Citations
Ceramic coating with high-temperature resistance and wear resistance and preparation method of ceramic coating
CN106007678A
Acid-resistant and heat-resistant inorganic anticorrosive coating and preparation method thereof
CN111074276A
Anti-corrosion and anti-coking ceramic coating convenient for state recognition and used for coal-fired boiler and preparation method of anti-corrosion and anti-coking ceramic coating
CN113999556A