Stone-like composite coating paint and preparation method thereof

By using cationic special modified emulsions and combinations of initiating crosslinking agents and heavy calcium and quartz sand in imitation stone coatings to form a crosslinked inner membrane, the problem of complexity and insufficient adhesion of traditional imitation stone coatings is solved. It has achieved simplification of construction technology and improved anti-saltitude and reduced costs.

CN119019904AActive Publication Date: 2024-11-26SKSHU PAINT
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411184681.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-26
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Traditional imitation stone paint has complicated construction processes, low construction efficiency, high labor costs, and high matching requirements between putty, primer, medium coating and imitation stone paint, which can easily lead to construction complexity and shedding problems.

Method used

Using cationic special modified emulsions, initiating crosslinking agents and compounded heavy calcium and quartz sand with a preferred mesh, the crosslinked inner membrane is formed through functional crosslinking, simplifying the construction process, improving adhesion and anti-saltitude resistance, Directly replace putty, primer, middle coating and imitation stone coating.

Benefits of technology

The construction process is greatly simplified, the construction cycle is shortened, the adhesion and crack resistance are enhanced, cracking and peeling problems caused by uncoupling between coatings, and the construction cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019904A_ABST
    Figure CN119019904A_ABST
Patent Text Reader

Abstract

The invention relates to a stone-like composite coating paint and a preparation method thereof, and the stone-like composite coating paint is mainly prepared from the following components in parts by weight: # imgabs0 #. The stone-like composite coating paint overcomes the defects of complicated construction process, low construction efficiency, high labor cost, low construction cost, low construction cost and the like of the traditional stone-like coating. In order to overcome the defects that in the prior art, in the prior art, a special cationic modified emulsion, an initiating cross-linking agent and compounded coarse whiting and quartz sand with preferable mesh numbers are adopted, and are in synergistic cooperation with other preferable components in a system and dosage proportions, so that the compatibility of putty, a primer, a floating coat and a stone-like coating is also required to a certain extent; the construction process is simple, the construction period is short, and the adhesive force, salt and alkali flooding resistance and cracking resistance are excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a stone-imitation composite coating paint and a preparation method thereof, and is applied in the field of stone-imitation coating production. Background Art

[0002] The statements in this section merely provide background information related to the present disclosure and may not constitute prior art.

[0003] With the improvement of people's economic level and the high-quality development of the construction industry, imitation stone coatings have been widely used in the market due to their advantages such as convenient construction, rich colors, water-based and environmentally friendly. However, the construction process of traditional imitation stone coatings is relatively complicated, with low construction efficiency and high labor costs. The specific process flow is as follows (see the coating structure for details) Figure 1 ): Base layer 1' (such as wall, etc.) treatment → scraping and applying flexible putty 1-2 times (putty layer 2') → rolling and applying sealing primer 1 time (primer layer 3') → rolling and applying intermediate paint 1-2 times (intermediate coating layer 4') → scraping or spraying imitation stone paint (imitation stone paint layer 5') → roller coating or spraying topcoat (topcoat layer 6'). Moreover, there are certain requirements for the compatibility between putty, primer, intermediate coating and imitation stone paint. Once the primer has poor sealing performance, the brushing is not in place, or the coatings do not match each other, the imitation stone paint may be lifted from the base layer and fall off.

[0004] Faced with the complexity of the above-mentioned multi-coating construction and the limitations of supporting equipment, relevant researchers have made certain improvements. For example, Chinese utility model patent CN 216865780 U proposes an indoor putty-free wall environmentally friendly coating structure. Although the utility model solves the problem of long leveling time and low efficiency of the putty layer by setting an adhesive layer, formaldehyde adsorption waterproof layer, wall cloth layer and paint brushing surface layer, it still requires multi-layer construction and paint brushing, and the construction process is relatively cumbersome; for example, Chinese invention patent CN 108250825 B proposes a black primer-free exterior wall putty and its preparation method. The putty not only has the functions of leveling, decoration, and sealing the substrate, but also achieves the effect of two processes in one process, reducing the material and labor costs, but the overall construction process also requires the construction of intermediate coating and imitation stone coating, which is only reduced by 1 / 4 compared with the traditional construction process.

[0005] Therefore, it is urgent to provide a stone-like composite coating paint with simple construction process, short construction period, excellent adhesion, anti-salinity and anti-cracking properties and a preparation method thereof. Summary of the invention

[0006] In order to overcome the shortcomings of traditional stone-like coatings, such as complicated construction procedures, low construction efficiency, high labor costs, and certain requirements on the compatibility of putty, primer, mid-coat and stone-like coating, the present invention provides a stone-like composite coating and a preparation method thereof, which adopts a preferred cationic special modified emulsion, an initiating cross-linking agent, and calcium carbonate and quartz sand compounded in preferred mesh sizes, and cooperates with other preferred components and dosage ratios in the system, and has the advantages of simple construction procedures, short construction period, excellent adhesion, anti-salinity and anti-cracking.

[0007] The technical solution of the present invention is as follows:

[0008] A stone-like composite coating is mainly prepared from the following components in the following weight ratios:

[0009]

[0010] The cationic special modified emulsion is mainly prepared from the following components in the following weight ratios:

[0011]

[0012] The crosslinking initiator is one or any combination of any two or more of polyethylene glycol diacrylate, N-hydroxymethyl acrylamide and diacetone acrylamide;

[0013] The heavy calcium carbonate is prepared by compounding 250-mesh heavy calcium carbonate and 500-mesh heavy calcium carbonate in a mass ratio of 2:1-6:1;

[0014] The quartz sand is prepared by compounding 40-80 mesh quartz sand and 80-120 mesh quartz sand in a mass ratio of 1:5-1:20.

[0015] The imitation stone composite coating of the present application adopts a preferred cationic special modified emulsion, an initiating crosslinking agent, and a preferred mesh compound of heavy calcium and quartz sand, and cooperates with other preferred components and dosage ratios in the system, and has the advantages of simple construction process, short construction period, excellent adhesion, anti-salinity and anti-cracking. Among them, the cationic special modified emulsion is prepared by acrylic esterification of epoxy polymer to obtain an unsaturated epoxy polymer intermediate, and then the unsaturated epoxy polymer intermediate, acrylic acid, styrene, butyl acrylate, and methyl methacrylate are used as monomers, and is prepared by cationic emulsion polymerization, and its minimum film forming temperature MFT is 3±2°C. The stone-like composite coating not only combines the five construction processes of putty, primer, mid-coat, stone-like topcoat and topcoat in the coating system of the traditional stone-like coating into one, greatly simplifies the construction process, shortens the construction period, and avoids the problems of cracking and falling off caused by the incompatibility between the coatings, but also specially introduces cationic positive charges (cationic special modified emulsion) into the formula system, and under the directional initiation of the preferred initiating cross-linking agent, functional cross-linking can be generated with the alkaline substance in the base layer, and a cross-linked inner film 2 (such as Figure 2 As shown), it plays the role of crack resistance, sealing, and barrier, so it has excellent water resistance and anti-salinity and anti-seepage. The advantages of the imitation stone composite coating are: (1) The imitation stone composite coating of the present application itself is a non-alkaline non-cement base and can be applied to the wall decoration of various buildings such as concrete, plaster base, thermal insulation base, etc.; (2) The coating system preferably uses a cationic special modified emulsion, which not only does not need to add a film-forming aid in the formula system, but also can be functionally cross-linked with the alkaline substances in the substrate to form a cross-linked inner film, which plays the role of sealing the substrate and has outstanding anti-salinity and anti-seepage performance; (3) In the system of this case, heavy calcium and quartz sand with specific mesh numbers and dosage ratios are preferably used to ensure the roughness of the lower surface of the imitation stone composite coating, and the bonding force between different bases is strong, avoiding the phenomenon of lifting from the base; (4) The imitation stone composite coating of this case can directly replace the putty, primer, intermediate paint, imitation stone paint and topcoat in the imitation stone coating construction system, which can greatly simplify the construction process, shorten the working time and reduce the cost.

[0016] The dispersing wetting agent is prepared by compounding a hydrophobically modified ammonium salt block copolymer and a nonionic surfactant in a mass ratio of 2:3-2:1.

[0017] The hydrophobically modified ammonium salt block copolymer and the nonionic surfactant both have outstanding water resistance, and using them in a preferred proportion can improve the water resistance and alkali resistance of the product.

[0018] The hydrophobic modified thickener is prepared by compounding a hydrophobic group-modified acrylic acid alkali swelling thickener and a nonionic associative thickener in a mass ratio of 2:3-2:5.

[0019] Compared with other thickeners, the hydrophobic group-modified acrylic alkali-swellable thickener and the nonionic associative thickener have excellent water resistance. Their use in a preferred proportion can make the paint film less likely to absorb water and have higher strength.

[0020] The stone-like composite coating paint also includes 0.1-3 parts of color paste.

[0021] The desired imitation stone decorative effect can be achieved by selecting the required color paste.

[0022] The color paste includes 0.05-2 parts of inorganic color paste and 0.05-1 part of organic color paste.

[0023] Inorganic colorants are cheap, have excellent weather resistance and high hiding power, but have low tinting strength and dark colors; organic colorants are bright in color and have high tinting strength, but are relatively expensive; the advantages of using the two together are complementary.

[0024] The quartz sand is natural white sand or natural colored sand.

[0025] The preferred quartz sand is widely available and low in cost.

[0026] The method for preparing the stone-like composite coating mainly comprises the following steps performed in sequence:

[0027] (1) Preparation of cationic special modified emulsion

[0028] ① Add triphenylphosphine to acrylic acid in a proportion of 1 / 6-1 / 5 of its total weight, and mix well to obtain an acrylic acid solution containing triphenylphosphine;

[0029] ② Start the stirrer and adjust the stirring speed to 300-400r / min, mix the epoxy resin and the remaining acrylic acid, stir evenly in a water bath at 85-90°C, then maintain the stirring speed, gradually drip the acrylic acid solution containing triphenylphosphine into the mixture while stirring to obtain a mixed solution; stop heating when the pH of the mixed solution is less than 5, and reduce the temperature to ≤50°C, thereby obtaining an unsaturated epoxy resin intermediate;

[0030] ③ Evenly mix butyl acrylate, methyl methacrylate, styrene and unsaturated epoxy resin to obtain a monomer mixture;

[0031] ④ Start the stirrer and adjust the stirring speed to 600-800r / min, mix 1 / 4-1 / 3 of the total weight of the gemini quaternary ammonium salt, 1 / 3-1 / 2 of the total weight of the alkylphenol polyoxyethylene ether and 1 / 3-1 / 2 of the total weight of the water, stir evenly in a 40-45°C water bath, then maintain the stirring speed, slowly add the monomer mixture while stirring, and continue stirring for 25-30 minutes to obtain a pre-emulsion;

[0032] ⑤ Start the stirrer and adjust the stirring speed to 200-300r / min, mix the remaining gemini quaternary ammonium salt, alkylphenol polyoxyethylene ether and water, add the pre-emulsion, stir evenly under 70-80°C water bath conditions, then maintain the stirring speed, add 1 / 6-1 / 5 of azobisisobutylamidine hydrochloride by weight while stirring to initiate the reaction, react for 0.4-0.6h, then add 1 / 6-1 / 5 of azobisisobutylamidine hydrochloride by weight every 0.4-0.6h until all the azobisisobutylamidine hydrochloride is added, keep warm for at least 1h after the addition is completed, then stop heating, and wait until the temperature drops to room temperature to obtain a cationic special modified emulsion;

[0033] (2) Add water to the disperser, start the disperser, and adjust the stirring speed to 400-500 rpm. Add a dispersing wetting agent, an antifreeze agent, and a defoaming agent to the disperser and disperse for 2-3 minutes. Then, maintain the stirring speed and slowly add the cationic special modified emulsion and disperse for another 3-5 minutes.

[0034] (3) Continue to add titanium dioxide, heavy calcium and quartz sand into the disperser, increase the stirring speed to 800-1000 rpm, and continue stirring until the system is free of agglomerates or particles;

[0035] (4) reducing the stirring speed to 700-800 rpm, continuing to add the bactericidal preservative, pH adjuster, initiator crosslinking agent and hydrophobic modified thickener into the disperser, stirring until the system is fully mixed, and then cooling to 23-25° C. to obtain the imitation stone composite coating.

[0036] The preparation method of the imitation stone composite coating paint in this case has simple steps and is easy to operate. The construction process of the imitation stone composite coating paint prepared by it is: base treatment → scraping 1-2 times of the imitation stone composite coating paint. It greatly simplifies the construction process of the existing imitation stone coating paint and shortens the construction period. It has strong adhesion with the base layer, excellent anti-salinity and anti-cracking properties, and can simultaneously meet the standard requirements of putty, primer, mid-coat, imitation stone coating and topcoat. Among them, in the step (1) of preparing the cationic special modified emulsion, the pH value is sampled and tested every 0.5h. The advantages of the preparation method of the imitation stone composite coating paint are: (1) it can be prepared by "one pot method", the steps are simple, the preparation is efficient, and it is easy to mass produce; (2) the imitation stone composite coating paint prepared in this case can directly replace the five processes of putty, primer, mid-coat, imitation stone coating and topcoat in the traditional imitation stone coating construction system, simplifying the construction process, shortening the working hours, and reducing the construction cost.

[0037] Step (4) of the method for preparing the stone-like composite coating paint also includes adding 0.1-3 parts of color paste.

[0038] Different imitation stone decorative effects can be achieved by adjusting the color of the color paste.

[0039] The color paste includes 0.05-2 parts of inorganic color paste and 0.05-1 part of organic color paste.

[0040] Compared with the prior art, the present invention has the following advantages:

[0041] 1) The imitation stone composite coating of the present application adopts a preferred cationic special modified emulsion, an initiating crosslinking agent, and a preferred mesh compound of heavy calcium and quartz sand, and cooperates with other preferred components and dosage ratios in the system, and has the advantages of simple construction process, short construction period, excellent adhesion, anti-salinity and anti-cracking;

[0042] 2) You can achieve the desired imitation stone decorative effect by selecting the required color paste;

[0043] 3) The preparation method of the stone-like composite coating in this case has simple steps, is easy to operate, can be prepared in a "one-pot method", has simple steps, is highly efficient in preparation, and is easy for large-scale production;

[0044] 4) The stone-like composite coating can directly replace the five processes of putty, primer, intermediate paint, stone-like paint and topcoat in the traditional stone-like coating construction system, simplifying the construction process, shortening the working hours and reducing the construction cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is a structural diagram of the construction of traditional imitation stone coating;

[0046] Figure 2The invention discloses a construction structure schematic diagram of the stone-like composite coating paint and a preparation method thereof.

[0047] Description of labels:

[0048] Base layer 1', putty layer 2', primer layer 3', middle coating layer 4', stone-like paint layer 5', topcoat layer 6', base layer 1, cross-linked inner film 2, stone-like composite coating paint layer 3. DETAILED DESCRIPTION

[0049] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments.

[0050] Example 1

[0051] The stone-like composite coating paint of the present invention is mainly prepared from the following components in the following weight ratios:

[0052]

[0053] 7 parts of hydrophobically modified thickener;

[0054] The cationic special modified emulsion is mainly prepared from the following components in the following weight ratios:

[0055]

[0056] The minimum film forming temperature MFT of the cationic special modified latex is 1°C.

[0057] The cross-linking initiator is polyethylene glycol diacrylate;

[0058] The heavy calcium carbonate is prepared by mixing 250-mesh heavy calcium carbonate and 500-mesh heavy calcium carbonate in a mass ratio of 2:1.

[0059] The quartz sand is compounded by mixing 40-80 mesh quartz sand and 80-120 mesh quartz sand in a mass ratio of 1:5.

[0060] The dispersing wetting agent is prepared by compounding a hydrophobically modified ammonium salt block copolymer and a nonionic surfactant in a mass ratio of 2:3.

[0061] The hydrophobic modified thickener is prepared by compounding a hydrophobic group-modified acrylic acid alkali swelling thickener and a nonionic associative thickener in a mass ratio of 2:3.

[0062] The stone-like composite coating paint also includes 1 part of organic color paste.

[0063] The quartz sand is natural white sand.

[0064] The method for preparing the stone-like composite coating mainly comprises the following steps performed in sequence:

[0065] (1) Preparation of cationic special modified emulsion

[0066] ① Add triphenylphosphine to acrylic acid accounting for 18% of its total weight, mix well, and obtain an acrylic acid solution containing triphenylphosphine;

[0067] ② Start the stirrer and adjust the stirring speed to 350r / min, mix the epoxy resin and the remaining acrylic acid, stir evenly in a water bath at 88°C, then maintain the stirring speed, gradually drop the acrylic acid solution containing triphenylphosphine into it while stirring to obtain a mixed solution; stop heating when the pH of the mixed solution is less than 5, and reduce the temperature to ≤50°C, thereby obtaining an unsaturated epoxy resin intermediate;

[0068] ③ Evenly mix butyl acrylate, methyl methacrylate, styrene and unsaturated epoxy resin to obtain a monomer mixture;

[0069] ④ Start the stirrer and adjust the stirring speed to 700r / min, mix 30% of the total weight of the gemini quaternary ammonium salt, 40% of the total weight of the alkylphenol polyoxyethylene ether and 40% of the total weight of the water, stir evenly in a 42°C water bath, then maintain the stirring speed, slowly add the monomer mixture while stirring, and continue stirring for 28 minutes to obtain a pre-emulsion;

[0070] ⑤ Start the stirrer and adjust the stirring speed to 250r / min, mix the remaining gemini quaternary ammonium salt, alkylphenol polyoxyethylene ether and water, add the pre-emulsion, stir evenly under 75°C water bath conditions, then maintain the stirring speed, add 18% of azobisisobutylamidine hydrochloride by weight while stirring to initiate the reaction, react for 0.5h, then add 18% of azobisisobutylamidine hydrochloride by weight every 0.5h until all the azobisisobutylamidine hydrochloride is added, keep warm for 1h after the addition is completed, then stop heating, and wait until the temperature drops to room temperature to obtain a cationic special modified emulsion;

[0071] (2) Add water to the disperser, start the disperser, and adjust the stirring speed to 400 rpm. Add the dispersing wetting agent, antifreeze agent and defoaming agent to the disperser and disperse for 2 minutes. Then, maintain the stirring speed and slowly add the cationic special modified emulsion and disperse for another 3 minutes.

[0072] (3) Continue to add titanium dioxide, heavy calcium and quartz sand into the disperser, increase the stirring speed to 800 rpm, and continue stirring until the system is free of agglomerates or particles;

[0073] (4) The stirring speed is reduced to 700 rpm, and the bactericidal preservative, pH adjuster, initiator crosslinking agent and hydrophobic modified thickener are continuously added into the disperser, and the mixture is stirred until the system is fully mixed and uniformly distributed, and then cooled to 24° C. to obtain a stone-like composite coating.

[0074] Step (4) of the method for preparing the stone-like composite coating paint also includes adding 1 part of organic color paste.

[0075] Example 2

[0076] The stone-like composite coating paint of the present invention is mainly prepared from the following components in the following weight ratios:

[0077]

[0078] The cationic special modified emulsion is mainly prepared from the following components in the following weight ratios:

[0079]

[0080]

[0081] The initiating crosslinking agent is N-hydroxymethyl acrylamide;

[0082] The heavy calcium carbonate is prepared by mixing 250-mesh heavy calcium carbonate and 500-mesh heavy calcium carbonate in a mass ratio of 3:1.

[0083] The quartz sand is prepared by compounding 40-80 mesh quartz sand and 80-120 mesh quartz sand in a mass ratio of 1:10.

[0084] The dispersing wetting agent is prepared by compounding a hydrophobically modified ammonium salt block copolymer and a nonionic surfactant in a mass ratio of 1:1.

[0085] The hydrophobically modified thickener is prepared by compounding a hydrophobic group-modified acrylic acid alkali swelling thickener and a nonionic associative thickener in a mass ratio of 1:2.

[0086] The stone-like composite coating paint also includes 1 part of inorganic color paste and 0.5 part of organic color paste.

[0087] The quartz sand is natural colored sand.

[0088] The method for preparing the stone-like composite coating mainly comprises the following steps performed in sequence:

[0089] (1) Preparation of cationic special modified emulsion

[0090] ① Add triphenylphosphine to acrylic acid in an amount of 1 / 6 of its total weight, and mix well to obtain an acrylic acid solution containing triphenylphosphine;

[0091] ② Start the stirrer and adjust the stirring speed to 400r / min, mix the epoxy resin and the remaining acrylic acid, stir evenly in a water bath at 85°C, then maintain the stirring speed, gradually drop the acrylic acid solution containing triphenylphosphine into the mixture while stirring to obtain a mixed solution; stop heating when the pH of the mixed solution is less than 5, and reduce the temperature to ≤50°C, thereby obtaining an unsaturated epoxy resin intermediate;

[0092] ③ Evenly mix butyl acrylate, methyl methacrylate, styrene and unsaturated epoxy resin to obtain a monomer mixture;

[0093] ④ Start the stirrer and adjust the stirring speed to 800r / min, mix the gemini quaternary ammonium salt accounting for 1 / 4 of the total weight ratio, the alkylphenol polyoxyethylene ether accounting for 1 / 2 of the total weight ratio and the water accounting for 1 / 3 of the total weight ratio, stir evenly in a 45°C water bath, then maintain the stirring speed, slowly add the monomer mixture while stirring, and continue stirring for 25 minutes to obtain a pre-emulsion;

[0094] ⑤ Start the stirrer and adjust the stirring speed to 300r / min, mix the remaining gemini quaternary ammonium salt, alkylphenol polyoxyethylene ether and water, add the pre-emulsion, stir evenly under 70°C water bath conditions, then maintain the stirring speed, add azobisisobutylamidine hydrochloride accounting for 1 / 5 of its total weight while stirring to initiate the reaction, react for 0.4h, then add azobisisobutylamidine hydrochloride accounting for 1 / 6 of its total weight every 0.6h until all the azobisisobutylamidine hydrochloride is added, continue to keep warm for 1.5h after the addition is completed, then stop heating, and wait until the temperature drops to room temperature to obtain a cationic special modified emulsion;

[0095] (2) Add water to the disperser, start the disperser, and adjust the stirring speed to 450 rpm. Add a dispersing wetting agent, an antifreeze agent, and a defoaming agent to the disperser and disperse for 2.5 minutes. Then, maintain the stirring speed and slowly add the cationic special modified emulsion and disperse for another 4 minutes.

[0096] (3) Continue to add titanium dioxide, heavy calcium and quartz sand into the disperser, increase the stirring speed to 900 rpm, and continue stirring until the system is free of agglomerates or particles;

[0097] (4) The stirring speed is reduced to 750 rpm, and the bactericidal preservative, pH adjuster, initiator crosslinking agent and hydrophobic modified thickener are continuously added into the disperser, and the mixture is stirred until the system is fully mixed and uniformly distributed, and then cooled to 23° C. to obtain a stone-like composite coating.

[0098] Step (4) of the method for preparing the stone-like composite coating paint also includes adding 1 part of inorganic color paste and 0.5 part of organic color paste.

[0099] Example 3

[0100] The stone-like composite coating paint of the present invention is mainly prepared from the following components in the following weight ratios:

[0101]

[0102] The cationic special modified emulsion is mainly prepared from the following components in the following weight ratios:

[0103]

[0104] 0.9 parts of azobisisobutylamidine hydrochloride;

[0105] The initiating crosslinking agent is diacetone acrylamide;

[0106] The heavy calcium carbonate is prepared by mixing 250-mesh heavy calcium carbonate and 500-mesh heavy calcium carbonate in a mass ratio of 6:1.

[0107] The quartz sand is prepared by compounding 40-80 mesh quartz sand and 80-120 mesh quartz sand in a mass ratio of 1:20.

[0108] The dispersing wetting agent is prepared by compounding a hydrophobically modified ammonium salt block copolymer and a nonionic surfactant in a mass ratio of 2:1.

[0109] The hydrophobically modified thickener is prepared by compounding a hydrophobic group-modified acrylic acid alkali swelling thickener and a nonionic associative thickener in a mass ratio of 2:5.

[0110] The stone-like composite coating paint also includes 2 parts of inorganic color paste.

[0111] The quartz sand is natural colored sand.

[0112] The method for preparing the stone-like composite coating mainly comprises the following steps performed in sequence:

[0113] (1) Preparation of cationic special modified emulsion

[0114] ① Add triphenylphosphine to acrylic acid in a proportion of 1 / 5 of its total weight, and mix well to obtain an acrylic acid solution containing triphenylphosphine;

[0115] ② Start the stirrer and adjust the stirring speed to 300r / min, mix the epoxy resin and the remaining acrylic acid, stir evenly in a 90°C water bath, then maintain the stirring speed, gradually drop the acrylic acid solution containing triphenylphosphine into the mixture while stirring to obtain a mixed solution; stop heating when the pH of the mixed solution is less than 5, and reduce the temperature to ≤50°C, thereby obtaining an unsaturated epoxy resin intermediate;

[0116] ③ Evenly mix butyl acrylate, methyl methacrylate, styrene and unsaturated epoxy resin to obtain a monomer mixture;

[0117] ④ Start the stirrer and adjust the stirring speed to 600r / min, mix the gemini quaternary ammonium salt accounting for 1 / 3 of the total weight ratio, the alkylphenol polyoxyethylene ether accounting for 1 / 3 of the total weight ratio and the water accounting for 1 / 2 of the total weight ratio, stir evenly in a 40°C water bath, then maintain the stirring speed, slowly add the monomer mixture while stirring, and continue stirring for 30 minutes to obtain a pre-emulsion;

[0118] ⑤ Start the stirrer and adjust the stirring speed to 200r / min, mix the remaining gemini quaternary ammonium salt, alkylphenol polyoxyethylene ether and water, add the pre-emulsion, stir evenly under 80°C water bath conditions, then maintain the stirring speed, add 1 / 6 of the total weight of azobisisobutylamidine hydrochloride dropwise while stirring to initiate the reaction, react for 0.6h, then add 1 / 5 of the total weight of azobisisobutylamidine hydrochloride dropwise every 0.4h until all the azobisisobutylamidine hydrochloride is added dropwise, continue to keep warm for 2h after the addition is completed, then stop heating, and wait until the temperature drops to room temperature to obtain a cationic special modified emulsion;

[0119] (2) Add water to the disperser, start the disperser, and adjust the stirring speed to 500 rpm. Add the dispersing wetting agent, antifreeze agent and defoaming agent to the disperser and disperse for 3 minutes. Then, maintain the stirring speed and slowly add the cationic special modified emulsion and disperse for another 5 minutes.

[0120] (3) Continue to add titanium dioxide, heavy calcium and quartz sand into the disperser, increase the stirring speed to 1000 rpm, and continue stirring until the system is free of agglomerates or particles;

[0121] (4) The stirring speed is reduced to 800 rpm, and the bactericidal preservative, pH adjuster, initiator crosslinking agent and hydrophobic modified thickener are continuously added into the disperser, and the mixture is stirred until the system is fully mixed and uniformly mixed, and then cooled to 25° C. to obtain a stone-like composite coating.

[0122] Step (4) of the method for preparing the stone-like composite coating paint also includes adding 2 parts of inorganic color paste.

[0123] Experimental data:

[0124] Comparative Example 1: The difference between this comparative example and Example 2 is that: the 250 mesh heavy calcium carbonate and the 500 mesh heavy calcium carbonate in Example 2 are replaced by equal amounts of 250 mesh heavy calcium carbonate; the 40-80 mesh quartz sand and the 80-120 mesh quartz sand in Example 2 are replaced by equal amounts of 80-120 mesh quartz sand.

[0125] Comparative Example 2: The difference between this comparative example and Example 2 is that the cationic special modified emulsion in Example 2 is replaced by an equal amount of ordinary pure acrylic emulsion, and no initiator crosslinking agent is added.

[0126] Detection method:

[0127] The following performance indicators are tested in accordance with JG / T 157-2009 "Putty for Building Exterior Walls", GB / T 9755-2014 "Synthetic Resin Emulsion Exterior Wall Paint" and JG / T 24-2018 "Synthetic Resin Emulsion Sand Wall Architectural Paint". If there are test methods for the same indicators, the test method with the highest test requirements shall be used for measurement.

[0128] The performance test results are shown in Table 1 below:

[0129] Table 1 Test results of comprehensive performance of coatings

[0130]

[0131]

[0132] As can be seen from Table 1, the imitation stone composite coating paints prepared in Examples 1-3 of this case all meet the various standard requirements of JG / T 157-2009 "Putty for Building Exterior Walls", GB / T 9755-2014 "Synthetic Resin Emulsion Exterior Wall Paint" and JG / T 24-2018 "Synthetic Resin Emulsion Sand Wall Building Paint", indicating that the imitation stone composite coating paint products of this case have excellent water seepage resistance, salt and alkali resistance, flexibility and excellent adhesion to the base layer. In addition, Comparative Examples 1-2 cannot meet the above three standard requirements at the same time. This shows that the preferred mesh size and dosage ratio of heavy calcium and quartz sand can form a certain rough surface to ensure adhesion to the substrate. At the same time, cationic positive charges are introduced into the formula system and under the directional initiation of the initiator cross-linking agent, functional cross-linking occurs with the alkaline substances in the base layer, forming a cross-linked inner film at the interface between the substrate and the stone-like composite coating, which plays a role in anti-crack sealing and barrier, so that the stone-like composite coating has excellent flexibility, water permeability and resistance to salt and alkali.

Claims

1. A stone-like composite coating, characterized in that: It is mainly prepared from the following components in the following weight ratios: The cationic special modified emulsion is mainly prepared from the following components in the following weight ratios: The cross-linking initiator is one or any combination of any two or more of polyethylene glycol diacrylate, N-hydroxymethyl acrylamide and diacetone acrylamide; The heavy calcium carbonate is prepared by compounding 250-mesh heavy calcium carbonate and 500-mesh heavy calcium carbonate in a mass ratio of 2:1-6:1; The quartz sand is prepared by compounding 40-80 mesh quartz sand and 80-120 mesh quartz sand in a mass ratio of 1:5-1:

20.

2. The stone-like composite coating according to claim 1, characterized in that: The dispersing wetting agent is prepared by compounding a hydrophobically modified ammonium salt block copolymer and a nonionic surfactant in a mass ratio of 2:3-2:

1.

3. The stone-like composite coating according to claim 1, characterized in that: The hydrophobically modified thickener is prepared by compounding a hydrophobic group-modified acrylic acid alkali swelling thickener and a nonionic associative thickener in a mass ratio of 2:3-2:

5.

4. The stone-like composite coating according to claim 1, characterized in that: The stone-like composite coating paint also includes 0.1-3 parts of color paste.

5. The stone-like composite coating according to claim 4, characterized in that: The color paste includes 0.05-2 parts of inorganic color paste and 0.05-1 part of organic color paste.

6. The stone-like composite coating according to claim 1, characterized in that: The quartz sand is natural white sand or natural colored sand.

7. The method for preparing the stone-like composite coating according to any one of claims 1 to 6, characterized in that: It mainly includes the following steps in order: (1) Preparation of cationic special modified emulsion ① Add triphenylphosphine to acrylic acid in a proportion of 1 / 6-1 / 5 of its total weight, mix well, and obtain an acrylic acid solution containing triphenylphosphine; ② Start the stirrer and adjust the stirring speed to 300-400r / min, mix the epoxy resin and the remaining acrylic acid, stir evenly in a water bath at 85-90°C, then maintain the stirring speed, gradually drip the acrylic acid solution containing triphenylphosphine into the mixture while stirring to obtain a mixed solution; stop heating when the pH of the mixed solution is less than 5, and reduce the temperature to ≤50°C, thereby obtaining an unsaturated epoxy resin intermediate; ③ Evenly mix butyl acrylate, methyl methacrylate, styrene and unsaturated epoxy resin to obtain a monomer mixture; ④ Start the stirrer and adjust the stirring speed to 600-800r / min, mix 1 / 4-1 / 3 of the total weight of the gemini quaternary ammonium salt, 1 / 3-1 / 2 of the total weight of the alkylphenol polyoxyethylene ether and 1 / 3-1 / 2 of the total weight of the water, stir evenly in a 40-45°C water bath, then maintain the stirring speed, slowly add the monomer mixture while stirring, and continue stirring for 25-30 minutes to obtain a pre-emulsion; ⑤ Start the stirrer and adjust the stirring speed to 200-300r / min, mix the remaining gemini quaternary ammonium salt, alkylphenol polyoxyethylene ether and water, add the pre-emulsion, stir evenly under 70-80°C water bath conditions, then maintain the stirring speed, add 1 / 6-1 / 5 of azobisisobutylamidine hydrochloride by weight while stirring to initiate the reaction, react for 0.4-0.6h, then add 1 / 6-1 / 5 of azobisisobutylamidine hydrochloride by weight every 0.4-0.6h until all the azobisisobutylamidine hydrochloride is added, keep warm for at least 1h after the addition is completed, then stop heating, and wait until the temperature drops to room temperature to obtain a cationic special modified emulsion; (2) Add water to the disperser, start the disperser, and adjust the stirring speed to 400-500 rpm. Add a dispersing wetting agent, an antifreeze agent, and a defoaming agent to the disperser and disperse for 2-3 minutes. Then, maintain the stirring speed and slowly add the cationic special modified emulsion and disperse for another 3-5 minutes. (3) Continue to add titanium dioxide, heavy calcium and quartz sand into the disperser, increase the stirring speed to 800-1000 rpm, and continue stirring until the system is free of agglomerates or particles; (4) reducing the stirring speed to 700-800 rpm, continuing to add the bactericidal preservative, pH adjuster, initiator crosslinking agent and hydrophobic modified thickener into the disperser, stirring until the system is fully mixed, and then cooling to 23-25° C. to obtain the imitation stone composite coating.

8. The method for preparing the stone-like composite coating according to claim 7 is characterized in that: Step (4) of the method for preparing the stone-like composite coating paint also includes adding 0.1-3 parts of color paste.

9. The method for preparing the stone-like composite coating according to claim 8 is characterized in that: The color paste includes 0.05-2 parts of inorganic color paste and 0.05-1 part of organic color paste.

Citation Information

Patent Citations

  • Preparation method of cationic acrylate epoxy resin

    CN102911344A

  • Corrosion-resistant and antibacterial cathode electrophoretic coating for railway fastener and coating method of coating

    CN103911058A

  • Colorful stone imitating coating and preparation method thereof

    CN109777223A

  • Waterborne epoxy stone-like coating and preparation method and application thereof

    CN110437700A

  • Slow-drying hard stone-like paint

    CN113861730A