High-performance water-based single-component imitation galvanized paint as well as preparation method and application thereof

Through the combination of LH-38X resin and zinc powder, the construction difficulty and performance problems of water-based imitation galvanized coatings are solved, and a water-based single-component imitation galvanized paint with high adhesion, salt spray resistance and environmental protection is achieved, suitable for steel surfaces Long-term anti-corrosion, replacing traditional hot-dip zinc and hot-spray zinc, providing better protection.

CN119019905AActive Publication Date: 2024-11-26ANQING LINGHU PAINT
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411292429.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-26
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

Most of the existing water-based imitation galvanized coatings are two-component products, which are difficult to mix evenly during construction, affect the performance of the coating and have low construction efficiency, and lack high-performance water-based single-component imitation galvanized paint.

Method used

Using the combination of LH-38X resin and zinc powder, through specific raw material ratios and preparation processes, high-performance aqueous single-component imitation galvanized paint, including methyl methacrylate, butyl acrylate, and methoxy polyethylene glycol Methacrylate, epoxy resin, silicone intermediate, etc., form resins with excellent adhesion and salt spray resistance through multi-step reaction, and add flash etching agent and anti-settling agent during construction to ensure dispersion and metals. Zinc content.

Benefits of technology

It achieves high adhesion, salt spray resistance and stability of the coating film, meets the long-term anti-corrosion needs of steel surfaces, replaces traditional hot-dip zinc and hot-spray zinc, provides better protection effects, and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005044999170000041
    Figure BDA0005044999170000041
  • Figure BDA0005044999170000051
    Figure BDA0005044999170000051
  • Figure BDA0005044999170000061
    Figure BDA0005044999170000061
Patent Text Reader

Abstract

The invention discloses a high-performance water-based single-component imitation galvanized paint, a preparation method and application. The paint is prepared from the following raw materials: LH-38X resin and zinc powder, the LH-38X resin is prepared from the following raw materials in parts by weight: 6 to 8 parts of methyl methacrylate, 5 to 7 parts of butyl acrylate, 1 to 3 parts of methoxy polyethylene glycol methacrylate, 1 to 3 parts of acrylic acid, 0.7 to 0.9 part of benzoyl peroxide, 0.3 to 0.5 part of n-dodecanethiol, 1 to 3 parts of organic silicon intermediate, 16 to 18 parts of epoxy resin, 2 to 4 parts of fatty acid, 0.2 to 0.4 part of tetrabutylammonium bromide and 0.03 to 0.1 part of zinc oxide. 3-5 parts of dimethylethanolamine, 0.8-1 part of a flash corrosion agent, 2-4 parts of an anti-settling agent and 52-58 parts of propylene glycol monomethyl ether. The adhesive force of the paint reaches 5 MPa, the salt mist resistance reaches 2000 h, the total zinc content is larger than 93%, the metal zinc content is larger than 90%, and the GB30981-2020 environmental protection requirement is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of paints, and in particular to a high-performance water-based single-component imitation zinc-plating paint and a preparation method and application thereof. Background Art

[0002] The cathodic protection effect of zinc powder in the imitation galvanizing paint makes the coating film have excellent corrosion resistance and has been widely used in metal protection. With the development of water-based coatings, the water-based imitation galvanizing paints currently sold on the market are basically two-component products. Due to the viscosity of the system, it is difficult to mix evenly during construction, which not only affects the performance of the coating film, but also has low construction efficiency. Water-based single-component imitation galvanizing paint is easy to apply, so the research and development of high-performance water-based single-component imitation galvanizing paint has broad market prospects. Summary of the invention

[0003] The technical problem to be solved by the present invention is how to obtain a single-component imitation zinc-plating paint with excellent performance.

[0004] The present invention solves the above technical problems through the following technical means:

[0005] A high-performance water-based one-component imitation zinc-plating paint, whose raw materials include LH-38X resin and zinc powder; the raw materials of the LH-38X resin include, by weight, 6-8 parts of methyl methacrylate, 5-7 parts of butyl acrylate, 1-3 parts of methoxy polyethylene glycol methacrylate, 1-3 parts of acrylic acid, 0.7-0.9 parts of benzoyl peroxide, 0.3-0.5 parts of n-dodecyl mercaptan, 1-3 parts of an organosilicon intermediate, 16-18 parts of an epoxy resin, 2-4 parts of a fatty acid, 0.2-0.4 parts of tetrabutylammonium bromide, 0.03-0.1 parts of zinc oxide, 3-5 parts of dimethylethanolamine, 0.8-1 parts of a flash etchant, 2-4 parts of an anti-settling agent, and 52-58 parts of propylene glycol methyl ether.

[0006] Preferably, the mass ratio of the LH-38X resin to the zinc powder is 14-16:84-86.

[0007] Preferably, the preparation method of the LH-38X resin comprises the following steps:

[0008] S1, methyl methacrylate, butyl acrylate, methoxy polyethylene glycol methacrylate, acrylic acid, n-dodecyl mercaptan and initiator benzoyl peroxide are mixed to prepare a monomer mixture; a portion of propylene glycol methyl ether is stirred and heated, and then the monomer mixture is added dropwise, and the mixture is reacted at the temperature to obtain an acrylate polymer;

[0009] S2, adding epoxy resin, fatty acid, tetrabutylammonium bromide and another part of propylene glycol methyl ether into a reaction device, heating and then keeping warm to react to obtain epoxy grafted product; during the keeping warm reaction, adding part of propylene glycol methyl ether to balance the temperature;

[0010] S3, adding epoxy grafted product, acrylate polymer, organosilicon intermediate, and zinc oxide into a reaction device, heating the reaction, cooling to room temperature after the reaction, adding another portion of propylene glycol methyl ether, and then adding dimethylethanolamine to obtain a mixed solution;

[0011] S4, mixing the above mixed solution with the flash etch agent and the anti-settling agent and dispersing them evenly, and then adding the remaining propylene glycol methyl ether to obtain the LH-38X resin.

[0012] Preferably, in S1, the monomer mixture is added dropwise after the temperature is raised to 95°C with stirring; the monomer mixture is added dropwise within 2-3 hours, and the temperature of the entire adding process is controlled at 100-105°C. After the addition is completed, the mixture is kept warm at 100-110°C for 3 hours; in S2, the temperature of the warm reaction is 110-120°C, and the reaction is carried out until the acid value is ≤1mgKOH / g; in S3, the temperature is raised to 110-120°C and the reaction is carried out until the acid value is ≤28mgKOH / g.

[0013] Preferably, the epoxy resin is epoxy resin E12; and the fatty acid is linoleic acid.

[0014] Preferably, the organosilicon intermediate is a condensation product of dimethylsiloxane and diphenylsiloxane.

[0015] Preferably, the flash etchant is a mixture of one or more of ZT703, ZT705, and ZT707 produced by Beijing Zhitu Chemical Co., Ltd.; the anti-settling agent is a mixture of one or two of BYK420 and BYK428 produced by BYK Chemical; and the zinc powder is 800-1000 mesh zinc powder.

[0016] Preferably, in S4, the dispersion is uniform in a disperser, the dispersion speed is 1500 r / min, and the dispersion time is 30 min.

[0017] The present invention also provides a method for preparing the high-performance water-based one-component imitation zinc-plating paint, comprising the following steps: uniformly mixing LH-38X resin and zinc powder to obtain the high-performance water-based one-component imitation zinc-plating paint.

[0018] Preferably, the preparation method of the high-performance water-based one-component imitation zinc-plating paint comprises the following steps: putting LH-38X resin into a batching device, adding zinc powder under stirring at 300 r / min, then adjusting the speed to 600-800 r / min, keeping stirring for 30 minutes, controlling the outlet material temperature to ≤50°C to obtain the high-performance water-based one-component imitation zinc-plating paint.

[0019] The invention also proposes an application of the high-performance water-based single-component imitation zinc-plating paint on a metal surface.

[0020] In the present invention, during the preparation process of LH-38X resin, one side of epoxy resin is firstly ring-opened with fatty acid, and then the other side of epoxy resin is ring-opened with carboxyl acrylate polymer, the carboxyl group in the carboxyl acrylate polymer is introduced into the acrylate prepolymer by acrylic acid, and the three are organically combined into an integral resin, the epoxy resin in the resin structure provides excellent adhesion, water resistance and salt spray resistance of the coating film, the aliphatic hydrocarbon long chain plays an internal plasticizing role, so that the high pigment-to-base ratio system has sufficient flexibility, and the double bonds contained are also easy to oxidatively polymerize, and the acrylate polymer part not only brings in carboxyl groups to ensure the water-based nature of the system, but also ensures the quick-drying characteristics of the film-forming process, which is conducive to the evaporation of water. Therefore, the coating film performance has both the flexibility of the aliphatic hydrocarbon long chain and the quick-drying and anti-aging characteristics of acrylic acid, and also has the excellent adhesion and salt spray resistance of epoxy resin, etc., and this organic combination can complement each other in terms of performance. The resin system does not contain water and also contains its own phase conversion catalyst tetrabutylammonium bromide, so it can be infinitely diluted with water without showing an obvious dilution peak.

[0021] In the present invention, during the preparation process of LH-38X resin, organosilicon chemistry is applied to acrylic epoxy polymerization, so that the generated product has the advantages of three materials at the same time. Since the organosilicon functional group Si-O bond is introduced into the resin, the anchoring group is anchored on the zinc powder, and the product of the invention has a barrier effect on water when diluted with water during the construction process. At the same time, the Si-O bond increases the cross-linking density of the coating film during the resin curing process, and accelerates the transformation of the resin from a linear polymer to a body structure. The organosilicon intermediate in the present invention is a condensation chain link of dimethylsiloxane and diphenylsiloxane, which has a small molecular weight, and the functional group is adsorbed on the surface of the zinc powder. During the dilution process of adding water during construction, it has a stabilizing effect on the zinc powder.

[0022] The high-performance water-based single-component imitation zinc-plating paint of the present invention requires salt spray resistance ≮2000h, adhesion ≮5MPa, total zinc content ≮93%, and metal zinc content ≮90%. In the late stage of resin synthesis, the flash etchant and the anti-settling agent are added to the resin, which not only ensures that the two have a high degree of dispersibility in the system, but also ensures that when the finished paint is produced, not only the total zinc content meets the requirements, but also the metal zinc content meets the requirements. If the process of adding the resin liquid, the flash etchant, the anti-settling agent, and the zinc powder in sequence is adopted, before the zinc powder is added, the system temperature is high and the air concentration is large, which can only ensure that the total zinc content meets the requirements, so the metal zinc content is always in a fluctuating state, sometimes falling to about 82-85%. Because the LH-38X resin system does not contain water, the paint formula adopts the mode of directly adding zinc powder to the LH-38X resin.

[0023] In the production process of the high-performance water-based single-component imitation galvanizing paint of the present invention, LH-38X resin is a key material for paint preparation, and the resin synthesis adopts an automatic temperature control device and a numerically controlled dropping instrument, thereby effectively controlling the reaction speed and polymerization time, and can make the molecular weight distribution of the synthetic resin narrower and the molecular weight moderate, ensuring that no obvious dilution peak appears, thereby also obtaining an ideal paint film; the selection of zinc powder is also very important, and the process of dispersing zinc powder in LH-38X resin is the final control of product quality to achieve satisfactory results.

[0024] Advantages of the present invention:

[0025] (1) The present invention adopts carboxyl-containing acrylic copolymer, long-chain aliphatic hydrocarbon monoacid, and organosilicon intermediate modified epoxy resin, and organically combines the substances into an integral resin, which has excellent film-forming property in water medium, good adhesion, and good salt spray resistance. The introduction of organosilicon intermediate enhances the stability of zinc powder in water-based system, solves the problem of coating film flexibility and wettability to zinc powder, solves the problem of water-based, and the characteristics of quick-drying film-forming, solves the characteristics of good adhesion and salt spray resistance and the stability of zinc powder, thereby ensuring the stability of the content of metallic zinc.

[0026] (2) The high-performance water-based single-component imitation galvanizing paint of the present invention is suitable for long-term corrosion protection of steel surfaces, replacing traditional hot-dip (galvanizing) galvanizing and hot-spraying galvanizing, achieving better protection effects than hot-dip (galvanizing) galvanizing and hot-spraying galvanizing, and can be used alone as a metal anti-corrosion protective layer and a heavy-duty anti-corrosion coating system primer, and can also be used to repair the damage caused by corrosion, welding, cutting, and riveting of various galvanized coatings on the surface of steel structures. It is widely used in the corrosion protection of various steel components and facilities, such as power transmission and transformation systems, power generation systems, bridge steel structures, concrete steel structures, steel structure buildings, marine facilities, high-speed railway and highway facilities, water conservancy facilities, civil air defense facilities, petrochemical equipment, etc.

[0027] (3) The high-performance water-based one-component imitation galvanizing paint of the present invention has an adhesion of 5MPa, a salt spray resistance of 2000h, a total zinc content of >93%, a metallic zinc content of >90%, and fully complies with the environmental protection requirements of GB30981-2020. It can be directly diluted with water during construction, which complies with environmental protection requirements. The resin system does not contain water, but water can be infinitely diluted without an obvious dilution peak. The VOC of the finished paint is 270-276g / L, which complies with VOC≤300g / L (GB30981-2020 Metal substrate protective coating one-component primer). DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0030] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0031] Example 1

[0032] Preparation of LH-38X resin used in high performance waterborne one-component imitation zinc coating

[0033] Raw materials used to synthesize LH-38X resin

[0034] 1.1 Material composition

[0035] Methyl methacrylate (MMA), butyl acrylate (BA), methoxy polyethylene glycol methacrylate (MPEG-MA), acrylic acid (AA), benzoyl peroxide (BPO), n-dodecyl mercaptan, epoxy resin (E12), fatty acid (linolenic acid with iodine value of 160-180 mgKOH / g, Anhui Ruifende Oil Deep Processing Co., Ltd.), tetrabutylammonium bromide, zinc oxide, silicone intermediate dimethylsiloxane and diphenylsiloxane condensation product (Dow Chemical), dimethylethanolamine, flash etching agent (Beijing Zhitu Chemical Co., Ltd. ZT703), anti-settling agent (BYK420), propylene glycol methyl ether, all are industrial products, zinc oxide is analytical grade.

[0036] 1.2 Weight parts of raw material components of LH-38X resin

[0037]

[0038]

[0039] 1.3LH-38X resin production process:

[0040] (1) Preparation of acrylic acid ester polymer

[0041] a. First, mix the formulated amounts of methyl methacrylate, butyl acrylate, methoxy polyethylene glycol methacrylate, acrylic acid, n-dodecyl mercaptan and initiator benzoyl peroxide to form a monomer mixture, and place it in a dropping kettle.

[0042] b. Add 1 / 4 part by weight of propylene glycol methyl ether as a base to a reaction kettle with a reflux device, start stirring, raise the temperature to 95°C, and start dripping the monomer mixture. The dripping should be completed within 2 hours. The temperature of the entire dripping process should be controlled at 100-105°C. After the dripping is completed, keep the temperature at 100-110°C for 3 hours to obtain an acrylate polymer.

[0043] (2) Preparation of epoxy grafted products

[0044] Add epoxy resin, fatty acid, tetrabutylammonium bromide and 1 / 3 weight part of propylene glycol methyl ether into a reaction kettle with a reflux device, heat until the epoxy resin melts, start stirring, and keep warm at 110-120°C for 2h. As the azeotropic point increases, add some propylene glycol methyl ether to balance the temperature. Take samples for acid value measurement after 2h. When the acid value is ≤1mgKOH / g, the reaction ends and the epoxy grafted product is obtained.

[0045] (3) Preparation of LH-38X resin

[0046] a. Add epoxy grafted product, acrylate polymer, silicone intermediate and zinc oxide into the reaction kettle, heat to 110-120℃ and keep for 2h. Take samples to measure the acid value after 2h. When the acid value is ≤28mgKOH / g, cool to room temperature, add part of propylene glycol methyl ether to reduce the viscosity, and then add dimethylethanolamine to neutralize the system pH value in the range of 7-9.

[0047] b. Transfer the obtained mixed solution into a high-speed disperser, add flashing agent and anti-settling agent in sequence, maintain the speed at 1500r / min for 30min, add the remaining propylene glycol methyl ether, and obtain LH-38X resin.

[0048] 1.4LH-38X resin test results

[0049]

[0050]

[0051] Example 2

[0052] Preparation of high performance water-based one-component zinc-plating paint

[0053] Main raw materials

[0054] 2.1 Material composition

[0055] The LH-38X resin and 800-mesh zinc powder prepared in Example 1. The 800-mesh zinc powder used in this example (purchased from Hunan Xinweiling Metal New Materials Technology Co., Ltd.) is an industrial product.

[0056] 2.2 The weight of each component of high-performance water-based one-component imitation galvanizing paint (kg) is:

[0057] LH-38X resin 14, zinc powder (800 mesh) 86.

[0058] 2.3 The preparation process of high-performance water-based one-component imitation zinc-plating paint is:

[0059] (1) Put LH-38X resin into the batching kettle, start the high-speed disperser, and add zinc powder while stirring slowly at 300r / min.

[0060] (2) After the zinc powder is added, adjust the speed to 600-800r / min, keep stirring for 30 minutes, stir evenly (the scraper is flat and there are no particles), and control the outlet material temperature ≤50℃. Stop stirring, filter and package to obtain a high-performance water-based one-component imitation zinc coating.

[0061] 2.4 Test results of high performance water-based one-component imitation galvanizing paint (refer to HG / T4845-2015 cold-coated zinc coating (oily))

[0062]

[0063]

[0064] Comparative Example 1

[0065] The only difference from Example 1 is:

[0066] 1.2 Weight parts of raw material components of LH-38X resin

[0067]

[0068] 1.3 In the production process of LH-38X resin, during the preparation of acrylate polymer, the dripping of b was completed in 2.5 hours.

[0069] Comparative Example 2

[0070] The only difference from Example 1 is:

[0071] 1.2 Weight parts of raw material components of LH-38X resin

[0072]

[0073] 1.3 In the production process of LH-38X resin, during the preparation of acrylate polymer, the dripping of b was completed within 3 hours.

[0074] Comparative Example In the preparation of LH-38X resin, the mass ratio of epoxy graft, acrylate polymer and silicone intermediate is different from that in Example 1, which will affect the coating performance of the product

[0075] Comparative Example 3

[0076] The resins prepared in Comparative Examples 1 and 2 were used to replace the resin in Example 2 to prepare coatings, and the coating film properties were compared as shown in the following table:

[0077] Test items Example 1 Comparative Example 1 Comparative Example 2 Metallic zinc content in non-volatile matter / %≥ 91.6 91.2 91.3 Total zinc content in non-volatile matter / %≥ 93.4 93.2 93.2 Adhesion (pull-off method) / MPa≥ 6.23 4.30 5.84 Salt spray resistance test / 2000h conform to 1200h 850h Surface dry min 20 15 20

[0078] From the above test results, it can be seen that the epoxy component is high, with good adhesion and salt spray resistance; the acrylic component is high and dries quickly, and the silicone component has a stabilizing effect on zinc powder.

[0079] Comparative Example 4

[0080] The only difference from Example 1 is that the raw material components of LH-38X resin do not contain methoxy polyethylene glycol methacrylate, and the acrylate polymer is prepared in a mass ratio of methyl methacrylate: butyl acrylate: acrylic acid: benzoyl peroxide: n-dodecyl mercaptan of 7:5.5:2:0.8:0.4; the epoxy graft is prepared in a mass ratio of epoxy resin: fatty acid: tetrabutylammonium bromide of 16.8:2.9:0.25; and the LH-38X resin is prepared while keeping the total content of the acrylate polymer unchanged, that is, in the preparation process of (3) LH-38X resin, the mass ratio of the acrylate polymer, the epoxy graft, and the silicone intermediate is the same as that in Example 1.

[0081] Comparative Example 5

[0082] The only difference from Example 1 is that the epoxy resin E18 is used instead of E12 in the raw material component of LH-38X resin, and the amount thereof is kept unchanged.

[0083] Comparative Example 6

[0084] The resins prepared in Comparative Examples 4 and 5 were used to replace the resin in Example 2 to prepare coatings, and the performance comparisons thereof are shown in the following table:

[0085]

[0086] From the above test results, it can be seen that if the MPEG-MA system is not used, the viscosity is large, the water solubility is poor, the drying property is poor, and the initial water resistance is poor; if the epoxy resin with a large epoxy value is replaced, the water solubility is poor, the drying property is poor, and the initial water resistance is poor.

[0087] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high-performance water-based one-component imitation zinc-plating paint, characterized in that: The raw materials include LH-38X resin and zinc powder; the raw materials of the LH-38X resin include, by weight, 6-8 parts of methyl methacrylate, 5-7 parts of butyl acrylate, 1-3 parts of methoxy polyethylene glycol methacrylate, 1-3 parts of acrylic acid, 0.7-0.9 parts of benzoyl peroxide, 0.3-0.5 parts of n-dodecyl mercaptan, 1-3 parts of organic silicon intermediate, 16-18 parts of epoxy resin, 2-4 parts of fatty acid, 0.2-0.4 parts of tetrabutylammonium bromide, 0.03-0.1 parts of zinc oxide, 3-5 parts of dimethylethanolamine, 0.8-1 parts of flash etchant, 2-4 parts of anti-settling agent and 52-58 parts of propylene glycol methyl ether.

2. The high performance water-based one-component imitation zinc-plating paint according to claim 1, characterized in that: The mass ratio of the LH-38X resin to the zinc powder is 14-16:84-86.

3. The high performance water-based one-component imitation zinc-plating paint according to claim 1, characterized in that: The preparation method of the LH-38X resin comprises the following steps: S1, methyl methacrylate, butyl acrylate, methoxy polyethylene glycol methacrylate, acrylic acid, n-dodecyl mercaptan and initiator benzoyl peroxide are mixed to prepare a monomer mixture; a portion of propylene glycol methyl ether is stirred and heated, and then the monomer mixture is added dropwise, and the mixture is reacted at the temperature to obtain an acrylate polymer; S2, adding epoxy resin, fatty acid, tetrabutylammonium bromide and another part of propylene glycol methyl ether into a reaction device, heating and then keeping warm to react to obtain epoxy grafted product; during the keeping warm reaction, adding part of propylene glycol methyl ether to balance the temperature; S3, adding epoxy grafted product, acrylate polymer, organosilicon intermediate, and zinc oxide into a reaction device, heating the reaction, cooling to room temperature after the reaction, adding another portion of propylene glycol methyl ether, and then adding dimethylethanolamine to obtain a mixed solution; S4, mixing the above mixed solution with the flash etch agent and the anti-settling agent and dispersing them evenly, and then adding the remaining propylene glycol methyl ether to obtain the LH-38X resin.

4. The high performance water-based one-component imitation zinc-plating paint according to claim 3, characterized in that: In S1, the monomer mixture is added dropwise after the temperature is raised to 95°C with stirring; the monomer mixture is added dropwise within 2-3 hours, and the temperature of the entire adding process is controlled at 100-105°C. After the addition is completed, the mixture is kept warm at 100-110°C for 3 hours; in S2, the temperature of the warm reaction is 110-120°C, and the reaction is carried out until the acid value is ≤1mgKOH / g; in S3, the temperature is raised to 110-120°C and the reaction is carried out until the acid value is ≤28mgKOH / g.

5. The high performance water-based one-component imitation zinc-plating paint according to claim 1, characterized in that: The epoxy resin is epoxy resin E12; the fatty acid is linoleic acid.

6. The high performance water-based one-component imitation zinc-plating paint according to claim 1, characterized in that: The organosilicon intermediate is a condensation product of dimethylsiloxane and diphenylsiloxane.

7. The high performance water-based one-component imitation zinc-plating paint according to any one of claims 1 to 6, characterized in that: The flash etchant is a mixture of one or more of ZT703, ZT705, and ZT707; the anti-settling agent is a mixture of one or two of BYK420 and BYK428; and the zinc powder is 800-1000 mesh zinc powder.

8. A method for preparing a high-performance water-based one-component imitation zinc-plating paint as claimed in any one of claims 1 to 7, characterized in that: The method comprises the following steps: uniformly mixing LH-38X resin and zinc powder to obtain the high-performance water-based single-component imitation zinc plating paint.

9. The method for preparing a high-performance water-based one-component imitation zinc-plating paint according to claim 8, characterized in that: The method comprises the following steps: putting LH-38X resin into a batching device, adding zinc powder under stirring at 300 r / min, adjusting the rotation speed to 600-800 r / min, maintaining stirring for 30 minutes, controlling the outlet material temperature to be ≤50°C, and discharging the material to obtain the high-performance water-based single-component imitation zinc-plating paint.

10. Use of the high-performance water-based one-component zinc-plating imitation paint according to any one of claims 1 to 7 on a metal surface.

Citation Information

Patent Citations

  • One-component room-temperature curing water-based anticorrosive resin and preparation method thereof

    CN108586678A

  • SH water-based acrylic acid modified epoxy ester and preparation method and application thereof

    CN111675953A

  • Hyperbranched epoxy zinc-rich coating and preparation method therefor

    WO2023035485A1