Anti-corrosion and fireproof integrated coating for building repair and preparation method of anti-corrosion and fireproof integrated coating
By using composite materials of anticorrosion coating and fire-resistant coating in building repairs, the integrated coating is formed, which solves the problem of single function of traditional coatings, and realizes the multiple efficient barrier effects of coatings and reduces construction complexity and cost. Effect.
Patent Information
- Application Number
- CN202411497750.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional anticorrosion coatings and fire-resistant coatings are mostly single functions, resulting in increased construction complexity and cost, making it difficult to achieve both corrosion and fire protection during building repairs.
Using composite materials with anticorrosion coating and fire-resistant coating, the anticorrosion coating and fire-resistant coating are prepared simultaneously, and combined with mixed materials to form an integrated coating, including anticorrosion composite materials, glass flakes, polysiloxanes, and nanometers Components such as silica, graphene oxide, and ammonium polyphosphate, activated carbon, expanded graphite, etc. combine stable composite materials and mixed materials to improve the overall performance of the coating.
The coating is achieved with multiple efficient barrier effects, which enhances hardness, adhesion, fire resistance and durability, reduces construction complexity and cost, and improves the mechanical and corrosion resistance of the coating.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building coatings, in particular to an anti-corrosion and fire-proof integrated coating for building repair and a preparation method thereof. Background Art
[0002] With the acceleration of urbanization and the extension of the service life of buildings, building repair has become increasingly important. Buildings are exposed to the natural environment for a long time, and are affected by wind, rain, ultraviolet rays, chemical corrosion and other factors, which are prone to aging, damage and other problems. Especially for some important public buildings and historical relics, maintenance and repair work is particularly critical.
[0003] In the process of building renovation, the application of anti-corrosion and fire-proof coatings is particularly important. Corrosion is one of the main problems faced by building materials (especially steel structures). Corrosion not only affects the beauty of buildings, but also seriously affects their structural safety. On the other hand, fire is a major hidden danger to building safety, especially in high-rise buildings and public places. Once a fire occurs, the consequences are disastrous. Therefore, in the process of building renovation, the demand for coatings that can provide both anti-corrosion and fire protection is particularly urgent.
[0004] At present, the anti-corrosion coatings and fire-retardant coatings on the market are mainly used separately, each with its own characteristics and application range. Anti-corrosion coatings mainly form a protective film to isolate corrosive media and delay the corrosion process, while fire-retardant coatings mainly expand when exposed to fire to form an insulating layer to prevent the spread of flames. However, traditional anti-corrosion coatings and fire-retardant coatings are mostly single-function and often require multiple layers of coating, which increases construction complexity and cost. Summary of the invention
[0005] In view of the problems existing in the existing anti-corrosion and fire-proof integrated coating for building repair and the preparation method thereof, the present invention is proposed.
[0006] Therefore, the problem to be solved by the present invention is that traditional anti-corrosion coatings and fire-retardant coatings are mostly single-function, and it is difficult to reduce the construction complexity and cost.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions: In a first aspect, an embodiment of the present invention provides an anti-corrosion and fire-proof integrated coating for building repair, wherein the integrated coating is a composite of an anti-corrosion coating and a fire-proof coating; The anti-corrosion coating comprises the following raw materials in parts by weight: Anticorrosive composite materials: 40-60 parts; Glass flakes: 25-45 parts; Polysiloxane: 15-20 parts; Nano silicon dioxide: 10-15 parts; Graphene oxide: 5-8 parts; The fire retardant coating comprises the following raw materials in parts by weight: Ammonium polyphosphate: 20-30 parts; Activated carbon: 10-15 parts; Expanded graphite: 5-10 parts; Stable composite material: 5-10 parts.
[0008] As a preferred solution of the anti-corrosion and fire-proof integrated coating for building repair of the present invention, the anti-corrosion composite material comprises the following raw materials in parts by weight: Zirconium silicate: 20-30 parts; Polyester resin: 16-21 parts; Carbon nanotubes: 2-5 parts; Dispersant: 1-2 parts; Adhesive: 1-2 parts.
[0009] As a preferred solution of the anticorrosion and fireproof integrated coating for building repair of the present invention, the stable composite material comprises the following raw materials in parts by weight: Phenolic resin: 2-4 parts; Silicate: 1.5-2 parts; Curing agent: 0.5-1.5 parts; Silica nanoparticles: 0.5-1.5 parts; Wetting agent: 0.5-1 part.
[0010] As a preferred embodiment of the anti-corrosion and fire-proof integrated coating for building repair described in the present invention, the curing agent is selected from any one or more combinations of hexamethylenetetramine, formic acid, melamine and formaldehyde.
[0011] As a preferred embodiment of the anticorrosive and fireproof integrated coating for building repair of the present invention, the wetting agent is selected from any one or more combinations of siloxanes, ethoxylates, phosphates and polyacrylates.
[0012] As a preferred embodiment of the anticorrosion and fireproof integrated coating for building repair of the present invention, the integrated coating further comprises a mixed material for adhering the anticorrosion coating and the fireproof coating; The mixed material comprises the following raw materials in parts by weight: Cellulose ether: 1-5 parts; Polyoxyethylene ether: 1-3 parts; Organoclay: 0.2-0.8 parts; Coupling agent: 0.1-0.5 parts.
[0013] In a second aspect, an embodiment of the present invention provides a method for preparing an integrated anti-corrosion and fire-proof coating for building repair, which comprises the following steps: Synchronously preparing the anti-corrosion coating and the fire-resistant coating; The anti-corrosion coating and the fire-proof coating are mixed with the mixed material to obtain an integrated anti-corrosion and fire-proof coating.
[0014] As a preferred embodiment of the method for preparing the anticorrosion and fireproof integrated coating for building repair of the present invention, when preparing the anticorrosion composite material, zirconium silicate, polyester resin, carbon nanotubes and dispersant are added into a disperser to obtain a dispersed mixture; Adding a binder to the dispersed mixture and putting the mixture into a mixer to obtain the anti-corrosion composite material; The dispersing machine is set at a speed of 1500-2000 rpm, a duration of 20-30 min, and a temperature of 20-35°C; The stirrer is set to a speed of 250-350 rpm, a duration of 20-30 min, and a temperature of 20-35° C.; The adhesive accounts for 0.6% to 2% of the anti-corrosion composite material; The preparation process of the anti-corrosion coating comprises: Add nano-silicon dioxide and graphene oxide to ethanol or water, and then use an ultrasonic disperser to disperse for 30 minutes to obtain a primary material; Add the anticorrosive composite material and polysiloxane into a disperser, set the speed to 1500-2000 rpm, and the time to 5-15 minutes to obtain a secondary material; Add glass flakes and secondary material into a blender and set the blending speed to 250-300 rpm for 15-30 minutes to obtain a tertiary material; Add the first-stage material to the third-stage material, continue mixing with a mixer, set the stirring speed to 250-300 rpm, and the duration to 30-40 minutes to obtain a finished material; The material to be finished is refined by a colloid mill, the rotation speed of the colloid mill is set to 3000 rpm, and the refining time is 20 minutes to obtain the anti-corrosion coating.
[0015] As a preferred embodiment of the method for preparing the anticorrosion and fireproof integrated coating for building repair of the present invention, when preparing the stable composite material, phenolic resin and silicate are added to a disperser, and the dispersion speed is set to 1200-1600 rpm for 15-30 min to obtain a primary mixture; Add the curing agent, wetting agent and the first-stage mixture into the mixer, set the stirring speed to 200prm for 30min to obtain the second-stage mixture; The silica nanoparticles and the secondary mixture were added to an ultrasonic disperser and set for 30 min to obtain a stable composite material; The preparation process of the fire retardant coating comprises: Add ammonium polyphosphate, activated carbon and expanded graphite to a disperser, set the dispersion speed to 1200-1600 rpm, and the duration to 15-30 min to obtain a three-stage mixture; The three-stage mixture is stirred by a stirrer, and a stable composite material is added, and the stirring speed is set to 150-300 rpm for 20-40 minutes to obtain a fire retardant coating.
[0016] As a preferred embodiment of the method for preparing the integrated anti-corrosion and fire-proof coating for building repair described in the present invention, the ratio of the anti-corrosion coating, the fire-proof coating and the mixed material is 8-10:4-6:0.5-1.5.
[0017] The beneficial effects of the present invention are: The use of anti-corrosion composite materials can enhance the hardness and strength of the coating, and further improve the adhesion and overall performance of the coating. Among them, zirconium silicate and carbon nanotubes can form a stable carbon layer structure with polyester resin, thereby playing a role in the fireproof performance of the coating. While achieving anti-corrosion, it can also increase the overall fireproofing. The flexibility and adhesion of polyester resin combined with the thermal stability and mechanical properties of zirconium silicate and carbon nanotubes can improve the durability and reliability of the coating.
[0018] The use of stable composite materials can further improve the strength and toughness of the coating and enhance the mechanical properties of the coating. Among them, phenolic resin and silicate both have excellent heat resistance, and the addition of silica nanoparticles can further improve the thermal stability of the composite material, allowing it to maintain its performance in high temperature environments.
[0019] The use of mixed materials enhances the mechanical strength and wear resistance of the coating, ensuring the durability of the coating under various harsh conditions. While providing adhesion, the combination of polyoxyethylene ether and cellulose ether enhances the anti-corrosion performance of the coating, forming a dense anti-corrosion barrier to prevent the penetration of corrosive media. DETAILED DESCRIPTION
[0020] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the following is a detailed description in conjunction with the specific implementation methods of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary persons in the art without creative work should fall within the scope of protection of the present invention.
[0021] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0022] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0023] In a first aspect, an embodiment of the present application provides an integrated anti-corrosion and fire-proof coating for building repair, wherein the integrated coating is a composite of an anti-corrosion coating and a fire-proof coating.
[0024] The anticorrosive coating comprises the following raw materials in parts by weight: Anticorrosive composite materials: 40-60 parts; Glass flakes: 25-45 parts; Polysiloxane: 15-20 parts; Nano silicon dioxide: 10-15 parts; Graphene oxide: 5-8 parts.
[0025] The anticorrosive composite material comprises the following raw materials in parts by weight: Zirconium silicate: 20-30 parts; Polyester resin: 16-21 parts; Carbon nanotubes: 2-5 parts; Dispersant: 1-2 parts; Adhesive: 1-2 parts; The use of zirconium silicate can enhance the hardness and strength of the coating. Polyester resin has good corrosion resistance, weather resistance and mechanical strength, and can improve the adhesion and overall performance of the coating. Carbon nanotubes have excellent shielding properties and can build multiple high-efficiency barriers inside the coating to effectively improve the shielding properties of the coating. Zirconium silicate and carbon nanotubes can form a stable carbon layer structure with polyester resin, thereby enhancing the fire resistance of the coating. The flexibility and adhesion of polyester resin combined with the thermal stability and mechanical properties of zirconium silicate and carbon nanotubes can improve the durability and reliability of the coating.
[0026] The fire retardant coating comprises the following raw materials in parts by weight: Ammonium polyphosphate: 20-30 parts; Activated carbon: 10-15 parts; Expanded graphite: 5-10 parts; Stable composite material: 5-10 parts.
[0027] The stabilized composite material comprises the following raw materials in parts by weight: Phenolic resin: 2-4 parts; Silicate: 1.5-2 parts; Curing agent: 0.5-1.5 parts; Silica nanoparticles: 0.5-1.5 parts; Wetting agent: 0.5-1 part; Silica nanoparticles can improve the strength and toughness of phenolic resin, and the addition of silicate further enhances the mechanical properties of the composite material. Both phenolic resin and silicate have excellent heat resistance. The addition of silica nanoparticles can further improve the thermal stability of the composite material, allowing it to maintain its performance in high temperature environments.
[0028] The curing agent is selected from any one or more combinations of hexamethylenetetramine, formic acid, melamine and formaldehyde; Through the use of curing agent, the curing process of phenolic resin can be optimized to ensure that the coating has good mechanical properties and chemical resistance. Secondly, the use of silica nanoparticles can promote the reaction between curing agent and resin, improve curing efficiency and final curing degree.
[0029] The wetting agent is selected from any one or more combinations of silicone, ethoxylate, phosphate ester and polyacrylate; The use of wetting agents can distribute other fillers more evenly and increase the mechanical properties of the coating. Secondly, wetting agents can improve the leveling of the coating, making it easier for the coating to form a smooth and uniform surface during construction.
[0030] Integrated coatings also include hybrid materials for adhesion of anti-corrosion coatings and fire-resistant coatings; The mixed material includes the following raw materials in parts by weight: Cellulose ether: 1-5 parts; Polyoxyethylene ether: 1-3 parts; Organoclay: 0.2-0.8 parts; Coupling agent: 0.1-0.5 parts; The combination of cellulose ether and organic clay enhances the mechanical strength and wear resistance of the coating, ensuring the durability of the coating under various harsh conditions. The combination of polyoxyethylene ether and cellulose ether enhances the anti-corrosion performance of the coating, forming a dense anti-corrosion barrier to prevent the penetration of corrosive media and form a heat insulation layer at high temperatures. The coupling agent increases the adhesion of each filler. Wherein, the coupling agent is y-aminopropyltriethoxysilane.
[0031] In a second aspect, the present application also provides a method for preparing an integrated anti-corrosion and fire-proof coating for building repair, comprising the following steps: Anti-corrosion coating and fire-retardant coating are prepared simultaneously.
[0032] When preparing the anticorrosive composite material, zirconium silicate, polyester resin, carbon nanotubes and a dispersant are added into a disperser to obtain a dispersed mixture; adding a binder to the dispersed mixture and putting the mixture into a mixer to obtain an anticorrosive composite material; The speed of the disperser is set to 1500-2000 rpm, the duration is 20-30 min, and the temperature is set to 20-35 ° C; The mixer is set to run at 250-350 rpm, for 20-30 min, and at a temperature of 20-35°C. Adhesives account for 0.6% to 2% of anti-corrosion composite materials; The preparation process of anti-corrosion coating includes: Add nano-silicon dioxide and graphene oxide to ethanol or water, and then use an ultrasonic disperser to disperse for 30 minutes to obtain a primary material; Add the anticorrosive composite material and polysiloxane into a disperser, set the speed to 1500-2000 rpm, and the time to 5-15 minutes to obtain a secondary material; Add glass flakes and secondary material into a blender and set the blending speed to 250-300 rpm for 15-30 minutes to obtain a tertiary material; Add the first-stage material to the third-stage material, continue mixing with a mixer, set the stirring speed to 250-300 rpm, and the duration to 30-40 minutes to obtain a finished material; The unfinished material is refined by a colloid mill, the rotation speed of the colloid mill is set to 3000 rpm, and the refining time is 20 minutes to obtain an anti-corrosion coating.
[0033] When preparing a stable composite material, phenolic resin and silicate are added to a disperser, and the dispersion speed is set to 1200-1600 rpm for 15-30 minutes to obtain a primary mixture; Add the curing agent, wetting agent and the first-stage mixture into the mixer, set the stirring speed to 200prm for 30min to obtain the second-stage mixture; The silica nanoparticles and the secondary mixture were added to an ultrasonic disperser and set for 30 min to obtain a stable composite material; The preparation process of fire retardant coating includes: Add ammonium polyphosphate, activated carbon and expanded graphite to a disperser, set the dispersion speed to 1200-1600 rpm, and the duration to 15-30 min to obtain a three-stage mixture; The three-stage mixture is stirred by a stirrer, and a stable composite material is added, and the stirring speed is set to 150-300 rpm for 20-40 minutes to obtain a fire retardant coating.
[0034] The anti-corrosion coating and the fire-proof coating are mixed with mixed materials to obtain an integrated anti-corrosion and fire-proof coating.
[0035] The ratio of anti-corrosion coating, fire-proof coating and mixed materials is 8-10:4-6:0.5-1.5. Example 1
[0036] The integrated coating of this embodiment includes the components shown in Table 1 below: Table 1: Integrated coating material list Element Added amount / portion Anti-corrosion composite materials 40 Glass flakes 25 Polysiloxane 15 Nano Silica 10 Graphene oxide 5 Ammonium Polyphosphate 20 Activated carbon 10 Expanded Graphite 5 Stabilizing composite materials 5 Mixed Materials 2.3 The anti-corrosion composite material includes the components shown in Table 2 below: Table 2: Anti-corrosion composite materials Element Added amount / portion Zirconium silicate 20 Polyester resin 16 Carbon Nanotubes 2 Dispersants 1 Adhesive 1 Wherein, the stable composite material includes the components shown in Table 3 below; Table 3: Table of stable composite materials Element Added amount / portion Phenolic resin 2 Silicate 1.5 Curing agent 0.5 Silica Nanoparticles 0.5 Wetting Agents 0.5 The mixed material includes the components shown in Table 4 below; Table 4: Mixed materials table Element Added amount / portion Cellulose ether 1 Polyoxyethylene ether 1 Organic Clay 0.2 Coupling agent 0.1 A combination of formic acid and melamine was used as a curing agent, and silicone was used as a wetting agent.
[0037] The preparation method of this embodiment is as follows: when preparing the anti-corrosion composite material, zirconium silicate, polyester resin, carbon nanotubes, and a dispersant are added into a disperser to obtain a dispersed mixture; adding a binder to the dispersed mixture and putting the mixture into a mixer to obtain an anticorrosive composite material; The speed of the disperser was set to 1500 rpm, the duration was 20 min, and the temperature was set to 20 °C; The mixer was set to a speed of 250 rpm, a duration of 20 min, and a temperature of 20 °C; The preparation process of anti-corrosion coating includes: Add nano-silicon dioxide and graphene oxide to ethanol or water, and then use an ultrasonic disperser to disperse for 30 minutes to obtain a primary material; Add the anticorrosive composite material and polysiloxane into a disperser, set the speed to 1500 rpm, and the duration to 5 min to obtain a secondary material; Add the glass flakes and the secondary material into the blender and set the blending speed to 250 rpm for 15 min to obtain the tertiary material; Add the first-level material to the third-level material, continue mixing with a mixer, set the stirring speed to 250 rpm, and the duration to 30 minutes to obtain a finished material; The unfinished material is refined by a colloid mill, the rotation speed of the colloid mill is set to 3000 rpm, and the refining time is 20 minutes to obtain an anti-corrosion coating.
[0038] When preparing the stable composite material, the phenolic resin and the silicate were added to the disperser, and the dispersion speed was set to 1200 rpm for 15 min to obtain a primary mixture; Add the curing agent, wetting agent and the first-stage mixture into the mixer, set the stirring speed to 200prm for 30min to obtain the second-stage mixture; The silica nanoparticles and the secondary mixture were added to an ultrasonic disperser and set for 30 min to obtain a stable composite material; The preparation process of fire retardant coating includes: Add ammonium polyphosphate, activated carbon and expanded graphite into a disperser, set the dispersion speed to 1200 rpm, and the duration to 15 min to obtain a three-stage mixture; The three-stage mixture was stirred by a stirrer, and the stabilizing composite material was added, and the stirring speed was set to 150 rpm for 20 min to obtain a fire retardant coating.
[0039] Example 2 The integrated coating of this embodiment includes the components shown in Table 5 below: Table 5: Integrated coating material table Element Added amount / portion Anti-corrosion composite materials 50 Glass flakes 35 Polysiloxane 17 Nano Silica 12 Graphene oxide 6 Ammonium Polyphosphate 25 Activated carbon 12 Expanded Graphite 7 Stabilizing composite materials 7 Mixed Materials 5.8 The anti-corrosion composite material includes the components shown in Table 6 below: Table 6: Anti-corrosion composite materials Element Added amount / portion Zirconium silicate 25 Polyester resin 18 Carbon Nanotubes 4 Dispersants 1.5 Adhesive 1.5 Wherein, the stable composite material includes the components shown in Table 7 below; Table 7: Table of stable composite materials Element Added amount / portion Phenolic resin 3 Silicate 1.5 Curing agent 1 Silica Nanoparticles 1 Wetting Agents 0.5 The mixed material includes the components shown in Table 8 below; Table 8: Mixed materials table Element Added amount / portion Cellulose ether 3 Polyoxyethylene ether 2 Organic Clay 0.5 Coupling agent 0.3 Hexamethylenetetramine was used as the curing agent, and ethoxylate was used as the wetting agent.
[0040] The preparation method is the same as that in Example 1.
[0041] Example 3 The integrated coating of this embodiment includes the components shown in Table 9 below: Table 9: Integrated coating material table Element Added amount / portion Anti-corrosion composite materials 60 Glass flakes 45 Polysiloxane 20 Nano Silica 15 Graphene oxide 8 Ammonium Polyphosphate 30 Activated carbon 15 Expanded Graphite 10 Stabilizing composite materials 10 Mixed Materials 9.3 The anti-corrosion composite material includes the components shown in Table 10 below: Table 10: Anti-corrosion composite materials Element Added amount / portion Zirconium silicate 30 Polyester resin 21 Carbon Nanotubes 5 Dispersants 2 Adhesive 2 Wherein, the stable composite material includes the components shown in Table 11 below; Table 11: Table of stable composite materials Element Added amount / portion Phenolic resin 4 Silicate 2 Curing agent 1.5 Silica Nanoparticles 1.5 Wetting Agents 1 The mixed material includes the components shown in Table 12 below; Table 12: Mixed materials table Element Added amount / portion Cellulose ether 5 Polyoxyethylene ether 3 Organic Clay 0.8 Coupling agent 0.5 Formaldehyde was used as the curing agent, and a combination of phosphate ester and polyacrylate was used as the wetting agent.
[0042] The preparation method of this embodiment is as follows: when preparing the anti-corrosion composite material, zirconium silicate, polyester resin, carbon nanotubes, and a dispersant are added into a disperser to obtain a dispersed mixture; adding a binder to the dispersed mixture and putting the mixture into a mixer to obtain an anticorrosive composite material; The speed of the disperser was set to 2000 rpm, the duration was 30 min, and the temperature was set to 35 °C; The mixer was set to a speed of 350 rpm, a duration of 30 min, and a temperature of 35 °C; The preparation process of anti-corrosion coating includes: Add nano-silicon dioxide and graphene oxide to ethanol or water, and then use an ultrasonic disperser to disperse for 30 minutes to obtain a primary material; Add the anticorrosive composite material and polysiloxane into a disperser, set the speed to 2000 rpm, and the duration to 15 min to obtain a secondary material; Add the glass flakes and the secondary material into the mixer and set the stirring speed to 300 rpm for 30 min to obtain the tertiary material; Add the first-level material to the third-level material, continue mixing with a mixer, set the stirring speed to 300 rpm, and the duration to 40 minutes to obtain a finished material; The unfinished material is refined by a colloid mill, the rotation speed of the colloid mill is set to 3000 rpm, and the refining time is 20 minutes to obtain an anti-corrosion coating.
[0043] When preparing the stable composite material, the phenolic resin and the silicate were added to the disperser, and the dispersion speed was set to 1600 rpm for 30 min to obtain a primary mixture; Add the curing agent, wetting agent and the first-stage mixture into the mixer, set the stirring speed to 200prm for 30min to obtain the second-stage mixture; The silica nanoparticles and the secondary mixture were added to an ultrasonic disperser and set for 30 min to obtain a stable composite material; The preparation process of fire retardant coating includes: Add ammonium polyphosphate, activated carbon and expanded graphite into a disperser, set the dispersion speed to 1200-1600 rpm, and the duration to 30 min to obtain a three-stage mixture; The three-stage mixture was stirred by a stirrer, and a stabilizing composite material was added. The stirring speed was set to 300 rpm for 40 min to obtain a fire retardant coating.
[0044] Comparative Example 1: No anti-corrosion composite material was used, and the remaining raw materials were the same as those of the anti-corrosion coating; Comparative Example 2: No stabilized composite material was used, and the remaining raw materials were the same as those of the fire retardant coating; Comparative Example 3: No mixed material was used, and the remaining raw materials were the same as those of the anti-corrosion coating and the fire-retardant coating; Table 13: Schematic diagram of integrated coating performance made with different ingredients
[0045] The adhesion test method is: using a cutting tool to cut the coating through the substrate in a right-angle grid pattern, and evaluating the resistance of the coating to detachment from the substrate. From the test results, none of Examples 1-3 showed any peeling, while the peeling area of the coating without using the stable composite material accounted for 15%, and the peeling area of the coating without using the mixed material accounted for 65%, which seriously affected normal use.
[0046] The test method of flexibility is: put the coating sample on the mold, gradually increase the pressure to deform the sample until the coating breaks. From the test results, the cupping value of Example 1 is 12mm, the cupping value of Example 2 is 11mm, and the cupping value of Example 3 is 12mm, all of which are in a non-crack state, the cupping value of Comparative Example 1 is 7mm, which is a slight crack, the cupping value of Comparative Example 2 is 5mm, which is a severe crack state, and the cupping value of Comparative Example 3 is 4mm, which is also a severe crack state.
[0047] The heat resistance detection method is: expose the coating to a set 150° environment for 3 hours, and then observe and record the appearance and performance changes of the coating. The result of Example 1 is that there is no obvious change in appearance and no change in hardness, so the heat resistance is high, the result of Example 2 is that there is no obvious change in appearance and no change in hardness, so the heat resistance is high, the result of Example 3 is that there is no obvious change in appearance and no change in hardness, so the heat resistance is high, the result of Comparative Example 1 is that the appearance is severely discolored and the hardness is slightly softened, so the heat resistance is poor, the result of Comparative Example 2 is that the appearance is slightly discolored and the hardness is slightly softened, so the heat resistance is medium, and the result of Comparative Example 3 is that the appearance is obviously discolored and the hardness is not changed, so the heat resistance is medium.
[0048] The anti-corrosion test method is: expose the coating to a salt spray test box, set the salt spray concentration to 5%, the test time to 72 hours, and the temperature to 40° C. The result of Example 1 is 0.09% corrosion area, the result of Example 2 is 0.11% corrosion area, the result of Example 3 is 0.08% corrosion area, the result of Comparative Example 1 is 1.6% corrosion area, the result of Comparative Example 2 is 0.7% corrosion area, and the result of Comparative Example 3 is 1.1% corrosion area.
[0049] The fire retardancy detection method is: place the coating in an experimental device, burn the coating with a flame, set the burning time to 1 minute, and observe the burning area of the flame. The result of Example 1 is 0.7% of the burning area, the result of Example 2 is 0.58% of the burning area, the result of Example 3 is 0.6% of the burning area, the result of Comparative Example 1 is 2.5% of the burning area, the result of Comparative Example 2 is 4.8% of the burning area, and the result of Comparative Example 3 is 1.9% of the burning area.
[0050] The aging resistance detection method is: expose the coating to a xenon lamp aging test box, set the light intensity to 0.6W / m², and test for 216 hours. The result of Example 1 is that the appearance is slightly faded, the tensile strength is unchanged, and the aging resistance is good. The result of Example 2 is that the appearance is slightly faded, the tensile strength is unchanged, and the aging resistance is good. The result of Example 3 is that the appearance is slightly faded, the tensile strength is unchanged, and the aging resistance is good. The result of Comparative Example 1 is that the appearance is slightly faded, the tensile strength is slightly decreased, and the aging resistance is medium. The result of Comparative Example 2 is that the appearance is slightly faded, the tensile strength is slightly decreased, and the aging resistance is medium. The result of Comparative Example 3 is that the appearance is slightly faded, the tensile strength is significantly decreased, and the aging resistance is poor.
[0051] In summary, the hardness and strength of the coating can be enhanced, and the adhesion and overall performance of the coating can be further improved. Among them, zirconium silicate and carbon nanotubes can form a stable carbon layer structure with polyester resin, thereby playing a role in the fireproof performance of the coating. While achieving anti-corrosion, the overall fireproofing is increased. The flexibility and adhesion of the polyester resin combined with the thermal stability and mechanical properties of zirconium silicate and carbon nanotubes can improve the durability and reliability of the coating.
[0052] The use of stable composite materials can further improve the strength and toughness of the coating and enhance the mechanical properties of the coating. Among them, phenolic resin and silicate both have excellent heat resistance, and the addition of silica nanoparticles can further improve the thermal stability of the composite material, allowing it to maintain its performance in high temperature environments.
[0053] The use of mixed materials enhances the mechanical strength and wear resistance of the coating, ensuring the durability of the coating under various harsh conditions. While providing adhesion, the combination of polyoxyethylene ether and cellulose ether enhances the anti-corrosion performance of the coating, forming a dense anti-corrosion barrier to prevent the penetration of corrosive media.
[0054] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. An integrated anticorrosion and fireproof coating for building repair, characterized in that: The integrated coating is a composite of an anti-corrosion coating and a fire-proof coating; The anti-corrosion coating comprises the following raw materials in parts by weight: Anticorrosive composite materials: 40-60 parts; Glass flakes: 25-45 parts; Polysiloxane: 15-20 parts; Nano silicon dioxide: 10-15 parts; Graphene oxide: 5-8 parts; The fire retardant coating comprises the following raw materials in parts by weight: Ammonium polyphosphate: 20-30 parts; Activated carbon: 10-15 parts; Expanded graphite: 5-10 parts; Stable composite material: 5-10 parts.
2. The anticorrosion and fireproofing integrated coating for building repair according to claim 1, characterized in that: The anti-corrosion composite material comprises the following raw materials in parts by weight: Zirconium silicate: 20-30 parts; Polyester resin: 16-21 parts; Carbon nanotubes: 2-5 parts; Dispersant: 1-2 parts; Adhesive: 1-2 parts.
3. The anticorrosion and fireproofing integrated coating for building repair according to claim 2, characterized in that: The stable composite material comprises the following raw materials in parts by weight: Phenolic resin: 2-4 parts; Silicate: 1.5-2 parts; Curing agent: 0.5-1.5 parts; Silica nanoparticles: 0.5-1.5 parts; Wetting agent: 0.5-1 part.
4. The anticorrosion and fireproofing integrated coating for building repair according to claim 3, characterized in that: The curing agent is selected from any one or more combinations of hexamethylenetetramine, formic acid, melamine and formaldehyde.
5. The anticorrosion and fireproofing integrated coating for building repair according to claim 4, characterized in that: The wetting agent is selected from any one or more combinations of silicone, ethoxylate, phosphate ester and polyacrylate.
6. The anticorrosion and fireproofing integrated coating for building repair according to claim 5, characterized in that: The integrated coating also includes a mixed material for adhering the anti-corrosion coating and the fire-proof coating; The mixed material comprises the following raw materials in parts by weight: Cellulose ether: 1-5 parts; Polyoxyethylene ether: 1-3 parts; Organoclay: 0.2-0.8 parts; Coupling agent: 0.1-0.5 parts.
7. A method for preparing an integrated anticorrosion and fireproof coating for building repair, characterized in that: The invention comprises the anticorrosion and fireproof integrated coating for building repair as claimed in claim 6, and the preparation method of the anticorrosion and fireproof integrated coating for building repair also comprises the following steps: Synchronously preparing the anti-corrosion coating and the fire-resistant coating; The anti-corrosion coating and the fire-proof coating are mixed with the mixed material to obtain an integrated anti-corrosion and fire-proof coating.
8. The method for preparing the anticorrosion and fireproof integrated coating for building repair according to claim 7, characterized in that: When preparing the anticorrosive composite material, zirconium silicate, polyester resin, carbon nanotubes and a dispersant are added into a disperser to obtain a dispersed mixture; Adding a binder to the dispersed mixture and putting the mixture into a mixer to obtain the anti-corrosion composite material; The dispersing machine is set at a speed of 1500-2000 rpm, a duration of 20-30 min, and a temperature of 20-35°C; The stirrer is set to a speed of 250-350 rpm, a duration of 20-30 min, and a temperature of 20-35° C.; The adhesive accounts for 0.6% to 2% of the anti-corrosion composite material; The preparation process of the anti-corrosion coating comprises: Add nano-silicon dioxide and graphene oxide to ethanol or water, and then use an ultrasonic disperser to disperse for 30 minutes to obtain a primary material; Add the anticorrosive composite material and polysiloxane into a disperser, set the speed to 1500-2000 rpm, and the time to 5-15 minutes to obtain a secondary material; Add glass flakes and secondary material into a blender and set the blending speed to 250-300 rpm for 15-30 minutes to obtain a tertiary material; Add the first-level material to the third-level material, continue mixing with a mixer, set the stirring speed to 250-300 rpm, and the duration to 30-40 minutes to obtain the finished material; The material to be finished is refined by a colloid mill, the rotation speed of the colloid mill is set to 3000 rpm, and the refining time is 20 minutes to obtain the anti-corrosion coating.
9. The method for preparing the anticorrosion and fireproofing integrated coating for building repair according to claim 8, characterized in that: When preparing the stable composite material, phenolic resin and silicate are added to a disperser, and the dispersion speed is set to 1200-1600 rpm for 15-30 minutes to obtain a primary mixture; Add the curing agent, wetting agent and the first-stage mixture into the mixer, set the stirring speed to 200prm for 30min to obtain the second-stage mixture; The silica nanoparticles and the secondary mixture were added to an ultrasonic disperser and set for 30 min to obtain a stable composite material; The preparation process of the fire retardant coating comprises: Add ammonium polyphosphate, activated carbon and expanded graphite to a disperser, set the dispersion speed to 1200-1600 rpm, and the duration to 15-30 min to obtain a three-stage mixture; The three-stage mixture is stirred by a stirrer, and a stable composite material is added, and the stirring speed is set to 150-300 rpm for 20-40 minutes to obtain a fire retardant coating.
10. The method for preparing the anticorrosion and fireproofing integrated coating for building repair according to claim 9, characterized in that: The ratio of the anti-corrosion coating, the fire-proof coating and the mixed material is 8-10:4-6:0.5-1.5.
Citation Information
Patent Citations
Metal protection paint, preparation method, application and hot-dip metal material
CN103788836A
Graphene waterborne industrial coating and preparation method thereof
CN105670474A
Graphene anticorrosive paint and preparation method thereof
CN111647342A
Water-based anti-scratch anticorrosive coating and preparation method thereof
CN113913094A