Spraying type low-cost high-film-thickness anti-cracking single-component water-based paint and preparation method thereof
By using a mixed water-based alkyd resin and drying agent in water-based spray-based products, the construction problems and high costs after the increase in water volume in the prior art are solved, and the high film thickness, crack resistance and weather resistance are improved. , reducing spraying costs and process time.
Patent Information
- Application Number
- CN202411284545.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-26
AI Technical Summary
The existing water-based spray-based products are difficult to meet the baking requirements after increasing the amount of water, which is costly and affects product promotion and can easily lead to thin and cracked spray films.
The preparation method of single-component water-based paint is adopted. By mixing different aqueous alkyd resins, drying agents and cosolvents, the viscosity and component ratio are adjusted to achieve high film thickness and crack resistance, and the spraying performance is increased during single spraying. The water volume reaches 70%, combined with self-emulsifying resin and thickener to ensure construction and weather resistance.
The paint film with high film thickness, crack resistance, high sagging, slow surface drying and fast hard work is achieved, which reduces spraying costs, improves water, acid and alkali resistance, salt spray resistance, and reduces process time and material waste.
Smart Images

Figure SMS_7 
Figure SMS_8 
Figure SMS_9
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water paint, and in particular to a spray-type low-cost, high-film-thickness, crack-resistant single-component water paint and a preparation method thereof. Background Art
[0003] Existing water-based spray products are used with a maximum of 20% water added to not affect the construction and use of the product. Adding too much water can easily lead to the existing construction failing to meet the baking and construction requirements, and the low cost affects the promotion of the product. Summary of the invention
[0004] In order to overcome the shortcomings of the prior art, the present invention provides a water-based paint that has high film thickness, resistance to cracking, high sag, slow surface drying, good actual drying, dense paint film and high gloss when the water amount is added to 70% of the total amount in a single spraying, lower spraying cost and excellent water resistance, acid and alkali resistance, and salt spray resistance.
[0005] On the one hand, the present invention provides a method for preparing a spray-type low-cost, high-film-thickness, crack-resistant, single-component water-based paint, comprising the following steps:
[0006] Add the first batch of water-based alkyd resin to the preparation pot, add amine neutralizer and stir at a speed of 500-600r / min; pre-mix the first batch of drying agent and environmentally friendly co-solvent and add them to the preparation pot, stir at a speed of 600-800r / min; add deionized water, the first defoamer, anti-rust filler, and pigment in succession, disperse them evenly, grind them until the fineness is not more than 25μm, then add the second batch of water-based alkyd resin, the second batch of drying agent and environmentally friendly co-solvent premix, the second defoamer, substrate wetting agent, and thickener in turn to mix the paint, stir at a speed of 900-1000r / min, and adjust the viscosity to Stormer viscosity 120ku.
[0007] In certain embodiments, the amine neutralizing agent is selected from DMEA.
[0008] In certain embodiments, the first batch of waterborne alkyd resin is selected from 3AK0211Y of Tongde Chemical, and the second batch of waterborne alkyd resin is selected from 3AK0235Y of Tongde Chemical.
[0009] In certain embodiments, the first batch of driers is a composite driers Troymax Kc10 and a zirconium carboxylate driers The second batch of driers is a composite driers TroymaxKc 10 and zirconium carboxylate driers A mixture of Zirconium 6.
[0010] In certain embodiments, the composite drier Troymax Kc 10 and the zirconium carboxylate drier Zirconium 6 has a weight ratio of 6.6:1.
[0011] In certain embodiments, the environmentally friendly co-solvent is CS-12 or CS-16.
[0012] In certain embodiments, the first batch of defoaming agent is selected from Digo Airex 901W, the second batch of defoamers is selected from BYK-024 of BYK Chemical; the substrate wetting agent is Digo Twin 4100.
[0013] In some embodiments, the thickener includes thickener 1 and thickener 2, wherein thickener 1 is an alkali swelling thickener Viscolam 330, and thickener 2 is a polyurethane low-alkali thickener. Gel 0620.
[0014] In certain embodiments, the anti-rust filler is a mixture of 1500-mesh barium sulfate and 1250-mesh talc powder in a weight ratio of 1:1; and the pigment is carbon black.
[0015] On the other hand, the present invention provides a spray-type low-cost, high-film-thickness, crack-resistant, single-component water-based paint, comprising the following components in weight percentage:
[0016]
[0017]
[0018] It is prepared by the following method:
[0019] Add the first batch of water-based alkyd resin to the preparation pot, add amine neutralizer and stir at a speed of 500-600r / min; pre-mix the first batch of drying agent and environmentally friendly co-solvent and add them to the preparation pot, stir at a speed of 600-800r / min; add deionized water, the first defoamer, anti-rust filler, and pigment in succession, disperse them evenly, grind them until the fineness is not more than 25μm, then add the second batch of water-based alkyd resin, the second batch of drying agent and environmentally friendly co-solvent premix, the second defoamer, substrate wetting agent, and thickener in turn to mix the paint, stir at a speed of 900-1000r / min, and adjust the viscosity to Stormer viscosity 120ku.
[0020] Compared with the prior art, the beneficial technical effects of the present invention are:
[0021] 1. Compared with traditional spray paint, it has the advantages of convenient construction, less consumption, lower cost, high film thickness and not easy to sag and crack;
[0022] 2. The prepared water-based paint dries slowly on the surface but dries quickly after spraying. It can be used directly on a warm substrate and can be baked in a shorter time, thus reducing process time and saving costs.
[0023] 3. Compared with traditional spray paint, it can stay in the machine for up to 8 hours, avoiding gun blockage and muzzle loss, and reducing the use of gun washing water.
[0024] 4. The present invention adopts two different water-based alkyd resins for mixing and uses carboxylic acid zirconium salt catalyst and composite cobalt catalyst in preparation, so that a synergistic effect is produced when the cobalt / zirconium molar ratio is 3, so that the cobalt drier accelerates the degradation of hydroperoxide, and the zirconium drier accelerates the polymerization of the compound and promotes the coordination between polymer segments, thereby accelerating the actual drying speed of the system; in addition, the coordination ability of the zirconium drier allows the polar groups on the polymer segments to alternate with each other, so that the viscosity and weight-average molecular weight of the system are increased; the system has high film thickness, crack resistance, high sag, slow surface drying, good actual drying, dense paint film and high gloss when the water amount added in a single spraying is 70% of the total amount, and has lower spraying cost and excellent water resistance, acid and alkali resistance, and salt spray resistance.
[0025] 5. Compared with the traditional technology, the invention produces thixotropy by combining the self-emulsifying resin and thickener, so that the paint still has thixotropy after adding a large amount of water to ensure workability. The self-emulsifying resin and solvent are combined with a drying agent to make the paint film dry slowly on the surface, dry quickly and resist cracking. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below through embodiments.
[0027] Example 1
[0028] A spray-type, low-cost, high-film-thickness, crack-resistant, one-component water-based paint comprises the following components in percentage by weight:
[0029]
[0030] It is prepared by the following method:
[0031] Add the first batch of water-based alkyd resin to the preparation pot, add amine neutralizer and stir at 500r / min for 5 minutes; pre-mix the first batch of drying agent and environmentally friendly co-solvent and add them to the preparation pot, stir at 600r / min for 10 minutes; add deionized water, the first defoamer, anti-rust filler and pigment successively, disperse them evenly and grind them until the fineness is not more than 25μm, then add the second batch of water-based alkyd resin, the second batch of drying agent and environmentally friendly co-solvent pre-mixture, the second defoamer, substrate wetting agent and thickener in turn to mix the paint, stir at 900r / min for 20 minutes, and adjust the viscosity to Stormer viscosity 120ku.
[0032] When using, add 70% ion water to the above water-based paint to reduce the viscosity to 31-35s.
[0033] Example 2
[0034] A spray-type, low-cost, high-film-thickness, crack-resistant, one-component water-based paint comprises the following components in percentage by weight:
[0035]
[0036] It is prepared by the following method:
[0037] Add the first batch of water-based alkyd resin to the preparation pot, add amine neutralizer and stir at a speed of 550r / min for 5min; pre-mix the first batch of drying agent and environmentally friendly co-solvent and add them to the preparation pot, stir at a speed of 700r / min for 10min; add deionized water, the first defoamer, anti-rust filler and pigment successively, disperse them evenly and grind them until the fineness is not more than 25μm, then add the second batch of water-based alkyd resin, the second batch of drying agent and environmentally friendly co-solvent pre-mixture, the second defoamer, substrate wetting agent and thickener in turn to mix the paint, stir at a speed of 950r / min for 20min, and adjust the viscosity to Stormer viscosity 120ku.
[0038] When using, add 70% ion water to the above water-based paint to reduce the viscosity to 31-35s.
[0039] Example 3
[0040] A spray-type, low-cost, high-film-thickness, crack-resistant, one-component water-based paint comprises the following components in percentage by weight:
[0041]
[0042]
[0043] It is prepared by the following method:
[0044] Add the first batch of water-based alkyd resin to the preparation pot, add amine neutralizer and stir at 600r / min for 5min; pre-mix the first batch of drying agent and environmentally friendly co-solvent and add them to the preparation pot, stir at 800r / min for 10min; add deionized water, the first defoamer, anti-rust filler and pigment successively, disperse them evenly and grind them until the fineness is not more than 25μm, then add the second batch of water-based alkyd resin, the second batch of drying agent and environmentally friendly co-solvent pre-mixture, the second defoamer, substrate wetting agent and thickener in turn to mix the paint, stir at 1000r / min for 20min, and adjust the viscosity to Stormer viscosity 120ku.
[0045] When using, add 70% ion water to the above water-based paint to reduce the viscosity to 31-35s.
[0046] Comparative Example 1
[0047] Commercially available spray-type one-component water-based paint.
[0048] The products of Examples 1-3 and Comparative Example 1 were subjected to performance tests, and the test results are shown in Table 1:
[0049] Table 1
[0050]
[0051]
[0052] In summary: the spray-type one-component water-based paint of the present invention has the following advantages:
[0053] 1. Compared with traditional spray paint, it has the advantages of convenient construction, less consumption, lower cost, high film thickness and not easy to sag and crack;
[0054] 2. The prepared water-based paint dries slowly on the surface but dries quickly after spraying. It can be used directly on a warm substrate and can be baked in a shorter time, thus reducing process time and saving costs.
[0055] 3. Compared with traditional spray paint, it can stay in the machine for up to 8 hours, avoiding gun blockage and muzzle loss, and reducing the use of gun washing water;
[0056] 4. The present invention adopts two different water-based alkyd resins for mixing and uses carboxylic acid zirconium salt catalyst and composite cobalt catalyst in preparation, so that a synergistic effect is produced when the cobalt / zirconium molar ratio is 3, so that the cobalt drier accelerates the degradation of hydroperoxide, and the zirconium drier accelerates the polymerization of the compound and promotes the coordination between polymer segments, thereby accelerating the actual drying speed of the system; in addition, the coordination ability of the zirconium drier allows the polar groups on the polymer segments to alternate with each other, so that the viscosity and weight-average molecular weight of the system are increased; the system has high film thickness, crack resistance, high sag, slow surface drying, good actual drying, dense paint film and high gloss when the water amount added in a single spraying is 70% of the total amount, and has lower spraying cost and excellent water resistance, acid and alkali resistance, and salt spray resistance.
[0057] 5. Compared with the traditional technology, the invention produces thixotropy by combining the self-emulsifying resin and thickener, so that the paint still has thixotropy after adding a large amount of water to ensure workability. The self-emulsifying resin and solvent are combined with a drying agent to make the paint film dry slowly on the surface, dry quickly and resist cracking.
[0058] The above description is only a preferred embodiment of the present invention. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the creative concept of the present invention, and these should also be regarded as within the scope of protection of the invention.
Claims
1. A method for preparing a spray-type low-cost, high-film-thickness, crack-resistant, one-component water-based paint, characterized in that: The steps include: Add the first batch of water-based alkyd resin to the preparation pot, add amine neutralizer and stir at a speed of 500-600r / min; pre-mix the first batch of drying agent and environmentally friendly co-solvent and add them to the preparation pot, stir at a speed of 600-800r / min; add deionized water, the first defoamer, anti-rust filler, and pigment in succession, disperse them evenly, grind them until the fineness is not more than 25μm, then add the second batch of water-based alkyd resin, the second batch of drying agent and environmentally friendly co-solvent premix, the second defoamer, substrate wetting agent, and thickener in turn to mix the paint, stir at a speed of 900-1000r / min, and adjust the viscosity to Stormer viscosity 120ku.
2. The method for preparing a spray-type low-cost, high-film-thickness, crack-resistant, one-component water-based paint according to claim 1, characterized in that: The amine neutralizing agent is selected from DMEA.
3. The method for preparing a spray-type low-cost, high-film-thickness, crack-resistant, one-component water-based paint according to claim 1, characterized in that: The first batch of waterborne alkyd resin is selected from 3AK0211Y of Tongde Chemical, and the second batch of waterborne alkyd resin is selected from 3AK0235Y of Tongde Chemical.
4. The method for preparing a spray-type low-cost, high-film-thickness, crack-resistant, one-component water-based paint according to claim 1, characterized in that: The first batch of driers is a composite driers Troymax Kc 10 and zirconium carboxylate driers The second batch of driers is a composite driers Troymax Kc 10 and zirconium carboxylate driers A mixture of Zirconium 6.
5. The method for preparing a spray-type low-cost, high-film-thickness, crack-resistant, one-component water-based paint according to claim 4, characterized in that: Composite drier Troymax Kc 10 and zirconium carboxylate drier Zirconium 6 has a weight ratio of 6.6:
1.
6. The method for preparing a spray-type low-cost, high-film-thickness, crack-resistant, one-component water-based paint according to claim 1, characterized in that: The environmentally friendly co-solvent is CS-12 or CS-16.
7. The method for preparing a spray-type low-cost, high-film-thickness, crack-resistant, one-component water-based paint according to claim 1, characterized in that: The first batch of defoamers is selected from Digo Airex 901, the second batch of defoamers is selected from BYK-024 of BYK Chemical; the substrate wetting agent is Digo Twin 4100.
8. The method for preparing a spray-type low-cost, high-film-thickness, crack-resistant, one-component water-based paint according to claim 1, characterized in that: The thickener includes thickener 1 and thickener 2, wherein thickener 1 is an alkali swelling thickener Viscolam 330, and thickener 2 is a polyurethane low-alkali thickener. Gel 0620.
9. The method for preparing a spray-type low-cost, high-film-thickness, crack-resistant, one-component water-based paint according to claim 1, characterized in that: The anti-rust filler is a mixture of 1500-mesh barium sulfate and 1250-mesh talc powder in a weight ratio of 1:1; the pigment is carbon black.
10. A spray-type, low-cost, high-film-thickness, crack-resistant, one-component water-based paint, prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The composition includes the following weight percentages:
Citation Information
Patent Citations
Special waterborne air-dried primer for bridges
CN106752788A
Water-borne rusty anticorrosive primer and preparation method thereof
CN109207034A
Water-based engineering machinery decoration finishing coat and preparation method thereof
CN109294418A
Water-based single-component anticorrosive primer and preparation method thereof
CN114621648A
Preparation method of dip-coating type single-component water-based paint
CN115820085A
Cited By
Rail transit vehicle axle surface water-based paint high film thickness one-time forming coating process
CN122828931A