Preparation method of wear-resistant modified waterborne polyurethane floor mortar coating

By introducing cationically modified graphene and sodium polyphenylsulfonate chain extender into water-based polyurethane floor mortar, the problem of insufficient hardness and wear resistance is solved, the hardness and antibacterial properties of the coating are improved, and better Floor application.

CN119019923AInactive Publication Date: 2024-11-26HANGZHOU JINGYUE BUILDING MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411140553.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Water-based polyurethane floor mortar coating has low hardness, poor wear resistance, and lacks antibacterial properties.

Method used

By introducing cationically modified graphene and sodium polyphenylsulfonate chain extender, surface modification and polymerization reaction are carried out to improve the dispersion and interface compatibility of graphene, and rigid benzene ring is introduced into the polyurethane molecular chain to enhance Hardness and wear resistance, while using cationic quaternary ammonium salt groups to enhance antibacterial properties.

Benefits of technology

It significantly improves the hardness and wear resistance of the paint film, reduces the wear per unit area, and gives polyurethane coatings strong antibacterial properties, making it better used in the field of floor mortar.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005000659330000021
    Figure BDA0005000659330000021
  • Figure BDA0005000659330000042
    Figure BDA0005000659330000042
  • Figure BDA0005000659330000051
    Figure BDA0005000659330000051
Patent Text Reader

Abstract

The invention belongs to the technical field of terrace mortar coatings, and discloses a preparation method of a wear-resistant modified waterborne polyurethane terrace mortar coating, which comprises the following steps: reacting polyester polyol, a sodium polyphenyl sulfonate chain extender and diisocyanate to obtain hydroxyl-terminated waterborne polyurethane, adding cationic modified graphene, a dispersing agent and color paste, and stirring to obtain the wear-resistant modified waterborne polyurethane terrace mortar coating. And adding polymethylene polyphenyl isocyanate to obtain the wear-resistant modified waterborne polyurethane floor mortar coating. The surface of graphene contains a large number of cationic quaternary ammonium salt groups, so that the graphene has strong bactericidal performance, and the antibacterial performance of the polyurethane coating can be improved. And the cationic quaternary ammonium salt can generate electrostatic interaction with sodium sulfonate anions in a polyurethane molecular chain, so that the interface bonding strength between graphene and polyurethane is enhanced, the graphene plays an excellent enhancement effect, and the hardness and wear resistance of the coating are remarkably improved. The polyurethane coating has good practical application in the field of floor mortar.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of floor mortar coatings, and in particular to a method for preparing a wear-resistant modified waterborne polyurethane floor mortar coating. Background Art

[0002] Floor mortar coatings are usually composed of resin, curing agent, cement mortar, pigment, etc. The resin matrix has a great influence on the performance of floor mortar coatings. The resin matrix mainly includes epoxy resin, polyurethane, polyurea resin, etc. Among them, water-based polyurethane is green and environmentally friendly, and has good toughness, heat resistance and durability. Improving the wear resistance, hardness, antibacterial and other properties of polyurethane resin is conducive to expanding the practical application of polyurethane in coatings, floor materials, etc.

[0003] Patent CN107434381B discloses a special floor coating waterborne polyurethane mortar composite coating and its preparation method and application. The waterborne polyurethane mortar composite coating prepared with polyols, isocyanate curing agents, alkaline earth metal hydroxides, etc. as raw materials has good mechanical properties, chemical corrosion resistance, antibacterial and mildew resistance, etc. However, the patent does not improve the wear resistance and other properties of the polyurethane mortar composite coating.

[0004] Patent CN117625031B discloses a method for preparing a wear-resistant and corrosion-resistant polyurethane self-leveling floor coating, which uses polyol, isocyanate curing agent, silicone phenolic resin modifier and the like as raw materials to improve the wear resistance, impact resistance and hardness of polyurethane. However, the patent does not give the polyurethane floor coating antibacterial and mildew-proof properties.

[0005] Graphene, as a nanomaterial with high strength, high hardness and good wear resistance, is widely used in polyurethane, coatings, floor cement mortar and other fields. However, graphene is prone to agglomeration and has poor dispersibility in materials such as polyurethane. It is not compatible with the material matrix. Therefore, it is necessary to modify the surface of graphene to enhance its compatibility with the material matrix. Summary of the invention

[0006] The invention solves the problems that the water-based polyurethane floor mortar coating has low hardness, poor wear resistance and no antibacterial property.

[0007] Technical solution: A method for preparing a wear-resistant modified waterborne polyurethane floor mortar coating:

[0008] Step A, add dry polyester polyol, sodium polyphenyl sulfonate chain extender, N,N-dimethylformamide solvent into a reaction kettle, introduce nitrogen, heat to 75-85°C, add diisocyanate and dibutyltin dilaurate, react for 3-4h, remove N,N-dimethylformamide solvent by vacuum distillation, add water, stir and disperse to obtain terminal hydroxyl waterborne polyurethane.

[0009] The sodium polyphenyl sulfonate chain extender has the structural formula (I) as follows:

[0010]

[0011] Step B, add terminal hydroxyl waterborne polyurethane and cationically modified graphene into a container, stir for 2-4 hours, add defoamer, dispersant, color paste, stir and disperse, and finally add polymethylene polyphenyl isocyanate to control the mass ratio of terminal hydroxyl waterborne polyurethane and cationically modified graphene to be 100:(0.2-2); obtain wear-resistant modified waterborne polyurethane floor mortar coating.

[0012] Furthermore, in step A, the molar ratio of the hydroxyl content of the polyester polyol, the sodium polyphenyl sulfonate chain extender, and the diisocyanate is (2.3-2.6):(1-1.2):1:(0.008-0.009).

[0013] Furthermore, the diisocyanate is hexamethylene diisocyanate, isophorone diisocyanate, or toluene diisocyanate.

[0014] Furthermore, the preparation method of the sodium polyphenyl sulfonate chain extender is as follows: toluene, 2,2'-sodium sulfonate-4,4'-diphenyl ether dicarboxylic acid, phenyl glycidyl ether, and tetrabutylammonium bromide in a molar ratio of 1:(2.2-2.6):(0.07-0.08) are added to a reaction bottle equipped with a condenser reflux tube, heated to 100-110° C., reacted for 8-12 hours, distilled under reduced pressure, washed with water and acetone, and then recrystallized in an ethanol aqueous solution with a volume fraction of 80% to obtain a sodium polyphenyl sulfonate chain extender.

[0015] Furthermore, the preparation method of the cation-modified graphene is as follows: treating graphene oxide in thionyl chloride, dispersing the obtained chlorinated graphene in dichloromethane, adding 1,3-di(dodecyl quaternary ammonium salt) propanol and triethylamine, and controlling the mass ratio of chlorinated graphene, 1,3-di(dodecyl quaternary ammonium salt) propanol, and triethylamine to be 100:(200-600):(40-180); stirring the reaction at room temperature for 18-36h, filtering, washing with water and ethanol in turn, and drying to obtain the cation-modified graphene.

[0016] Furthermore, the wear-resistant modified waterborne polyurethane floor mortar coating is used in floor mortar.

[0017] Technical effect: The present invention reacts the acyl chloride group of acyl chloride graphene with the hydroxyl group of 1,3-di(dodecyl quaternary ammonium salt) propanol to obtain cation-modified graphene, thereby introducing a large number of cationic quaternary ammonium salt groups on the surface of graphene, thereby achieving organic surface modification of graphene.

[0018] The invention carries out a ring-opening reaction on 2,2'-sodium sulfonate-4,4'-diphenyl ether dicarboxylic acid and phenyl glycidyl ether to obtain a novel sodium polyphenyl sulfonate chain extender, which is then polymerized and chain extended with polyester polyol and diisocyanate to obtain a sodium sulfonate type waterborne polyurethane. The sodium polyphenyl sulfonate chain extender contains a large number of rigid benzene rings, which are introduced into the polyurethane molecular chain, thereby facilitating the improvement of the hardness and wear resistance of the polyurethane.

[0019] The present invention compounds sodium sulfonate type waterborne polyurethane with cationic modified graphene, defoamer, color paste and other additives to obtain wear-resistant modified waterborne polyurethane floor mortar coating. After the surface of graphene is organically modified, the dispersibility is better and it is not easy to agglomerate in the waterborne polyurethane coating. In addition, the surface of graphene contains a large number of cationic quaternary ammonium salt groups, which can have strong bactericidal performance and improve the antibacterial performance of the polyurethane coating.

[0020] The cationic quaternary ammonium salt on the surface of the graphene of the present invention can electrostatically interact with the sodium sulfonate anions in the polyurethane molecular chain, further enhancing the interfacial bonding strength between the graphene and the polyurethane, so that the graphene can exert an excellent reinforcing effect, significantly improve the hardness of the paint film, reduce the wear amount per unit area, and improve the wear resistance. The polyurethane coating has good practical application in the field of floor mortar. DETAILED DESCRIPTION

[0021] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0022] 1,3-di(dodecyl quaternary ammonium salt) propanol was prepared according to the method of the master's thesis "Preparation of polyurethane-based damping coating materials for the synthesis of new organosilicon diquaternary ammonium salts and organosilicon antibacterial drugs".

[0023] Add 6.57g 1,3-dichloropropanol, 22.41g N,N-dimethyldodecylamine, and 20g n-propanol to a reaction bottle equipped with a condenser reflux tube, heat to 95°C, react for 12h, distill under reduced pressure, add ethyl acetate, heat and stir to dissolve, cool and recrystallize to obtain 1,3-di(dodecyl quaternary ammonium salt)propanol. The structural formula is

[0024] 2,2'-Sodium sulfonate-4,4'-diphenyl ether dicarboxylic acid was prepared according to the method of Journal of Polymer Science: Part A: Polymer Chemistry, Vol. 48, 1732-1742; "Synthesis and characterization of ionic conducting sulfonated polybenzimidazoles".

[0025] Introduce nitrogen into a reaction bottle equipped with a condenser reflux tube, add 150mL 30% fuming sulfuric acid (SO3 free amount 30%), 75g 4,4'-diphenyl ether dicarboxylic acid, heat to 110°C, react for 2h, and after cooling, pour the solution into a saturated sodium chloride solution. After filtering, the precipitate is recrystallized in water to obtain 2,2'-sodium sulfonate-4,4'-diphenyl ether dicarboxylic acid. The structural formula is:

[0026] To a reaction bottle equipped with a condenser reflux tube, 40 mL of thionyl chloride and 0.5 g of graphene oxide were added, nitrogen was introduced after ultrasonication, the reaction was heated to 70°C, the reaction was carried out for 24 hours, vacuum distillation was performed, and the acetone was washed to obtain chlorinated graphene.

[0027] Example 1

[0028] (1) Add 60 mL of dichloromethane, 0.5 g of chlorinated graphene, 3 g of 1,3-di(dodecyl quaternary ammonium salt)propanol, and 0.9 g of triethylamine to a reaction bottle; stir and react at room temperature for 36 hours, filter, wash with water and ethanol in turn, and dry to obtain cation-modified graphene.

[0029] (2) Add 250 mL of toluene, 60 mmol of 2,2'-sodium sulfonate-4,4'-diphenyl ether dicarboxylic acid, 156 mmol of phenyl glycidyl ether, and 4.2 mmol of tetrabutylammonium bromide to a reaction bottle equipped with a condenser reflux tube, heat to 100°C, react for 12 hours, distill under reduced pressure, wash with water and acetone, and then recrystallize in an ethanol aqueous solution with a volume fraction of 80% to obtain a sodium polyphenyl sulfonate chain extender. Preparation reaction formula:

[0030]

[0031] (3) Add dried polyester polyol 2000 with a hydroxyl content of 260 mmol, 110 mmol sodium polyphenyl sulfonate chain extender, and 50 mL N, N-dimethylformamide solvent to the reactor, introduce nitrogen, heat to 80°C, add 100 mmol hexamethylene diisocyanate and 0.9 mmol dibutyltin dilaurate, react for 3 hours, remove the N, N-dimethylformamide solvent by vacuum distillation, add 800 mL water, stir and disperse, and obtain a hydroxyl-terminated waterborne polyurethane.

[0032] (4) Add 1000g of hydroxyl-terminated waterborne polyurethane and 2g of cationic modified graphene into a container, stir for 2h, then add 7.2g of defoamer RhodoLine DF 6002, 9.7g of dispersant BYK-2013, and 120g of waterborne bright red slurry, stir and disperse, and finally add 210g of polymethylene polyphenyl isocyanate to obtain a wear-resistant modified waterborne polyurethane floor mortar coating.

[0033] Example 2

[0034] (1) Add 60 mL of dichloromethane, 0.5 g of chlorinated graphene, 2.3 g of 1,3-di(dodecyl quaternary ammonium salt)propanol, and 0.7 g of triethylamine to a reaction flask; stir and react at room temperature for 36 hours, filter, wash with water and ethanol in turn, and dry to obtain cation-modified graphene.

[0035] (2) Add 300 mL of toluene, 60 mmol of 2,2'-sodium sulfonate-4,4'-diphenyl ether dicarboxylic acid, 156 mmol of phenyl glycidyl ether, and 4.2 mmol of tetrabutylammonium bromide to a reaction bottle equipped with a condenser reflux tube, heat to 100° C., react for 8 hours, distill under reduced pressure, wash with water and acetone, and then recrystallize in an ethanol aqueous solution with a volume fraction of 80% to obtain a sodium polyphenyl sulfonate chain extender.

[0036] (3) Add dried polyester polyol 2000 with a hydroxyl content of 230 mmol, 120 mmol sodium polyphenyl sulfonate chain extender, and 50 mL N, N-dimethylformamide solvent into the reactor, introduce nitrogen, heat to 75°C, add 100 mmol toluene diisocyanate and 0.8 mmol dibutyltin dilaurate, react for 4 hours, remove the N, N-dimethylformamide solvent by vacuum distillation, add 800 mL of water, stir and disperse, and obtain a hydroxyl-terminated waterborne polyurethane.

[0037] (4) Add 1000 g of hydroxyl-terminated waterborne polyurethane and 8 g of cationic modified graphene into a container, stir for 2 h, add 7.2 g of defoamer RhodoLine DF 6002, 9.7 g of dispersant BYK-2013, and 120 g of waterborne bright red slurry, stir and disperse, and finally add 210 g of polymethylene polyphenyl isocyanate to obtain a wear-resistant modified waterborne polyurethane floor mortar coating.

[0038] Example 3

[0039] (1) Add 50 mL of dichloromethane, 0.5 g of chlorinated graphene, 1.6 g of 1,3-di(dodecyl quaternary ammonium salt)propanol, and 0.5 g of triethylamine to a reaction flask; stir and react at room temperature for 24 h, filter, wash with water and ethanol in turn, and dry to obtain cation-modified graphene.

[0040] (2) Add 250 mL of toluene, 60 mmol of 2,2'-sodium sulfonate-4,4'-diphenyl ether dicarboxylic acid, 132 mmol of phenyl glycidyl ether, and 4.8 mmol of tetrabutylammonium bromide to a reaction bottle equipped with a condenser reflux tube, heat to 110° C., react for 12 hours, distill under reduced pressure, wash with water and acetone, and then recrystallize in an ethanol aqueous solution with a volume fraction of 80% to obtain a sodium polyphenyl sulfonate chain extender.

[0041] (3) Add dried polyester polyol 2000 with a hydroxyl content of 240 mmol, 110 mmol sodium polyphenyl sulfonate chain extender, and 50 mL N, N-dimethylformamide solvent to the reactor, introduce nitrogen, heat to 85°C, add 100 mmol isophorone diisocyanate and 0.8 mmol dibutyltin dilaurate, react for 3 hours, remove the N, N-dimethylformamide solvent by vacuum distillation, add 800 mL water, stir and disperse, and obtain a hydroxyl-terminated waterborne polyurethane.

[0042] (4) Add 1000 g of hydroxyl-terminated waterborne polyurethane and 14 g of cationic modified graphene into a container, stir for 4 h, add 7.2 g of defoamer RhodoLine DF 6002, 9.7 g of dispersant BYK-2013, and 120 g of waterborne bright red slurry, stir and disperse, and finally add 210 g of polymethylene polyphenyl isocyanate to obtain a wear-resistant modified waterborne polyurethane floor mortar coating.

[0043] Example 4

[0044] (1) Add 50 mL of dichloromethane, 0.5 g of chlorinated graphene, 1 g of 1,3-di(dodecyl quaternary ammonium salt)propanol, and 0.2 g of triethylamine to a reaction flask; stir and react at room temperature for 18 h, filter, wash with water and ethanol in turn, and dry to obtain cation-modified graphene.

[0045] (2) Add 300 mL of toluene, 60 mmol of 2,2'-sodium sulfonate-4,4'-diphenyl ether dicarboxylic acid, 148 mmol of phenyl glycidyl ether, and 4.2 mmol of tetrabutylammonium bromide to a reaction bottle equipped with a condenser reflux tube, heat to 110° C., react for 10 hours, distill under reduced pressure, wash with water and acetone, and then recrystallize in an ethanol aqueous solution with a volume fraction of 80% to obtain a sodium polyphenyl sulfonate chain extender.

[0046] (3) Add dried polyester polyol 2000 with a hydroxyl content of 260 mmol, 100 mmol sodium polyphenyl sulfonate chain extender, and 50 mL N,N-dimethylformamide solvent to the reactor, introduce nitrogen, heat to 85°C, add 100 mmol toluene diisocyanate and 0.9 mmol dibutyltin dilaurate, react for 3 hours, remove the N,N-dimethylformamide solvent by vacuum distillation, add 800 mL of water, stir and disperse, and obtain a hydroxyl-terminated waterborne polyurethane.

[0047] (4) Add 1000 g of hydroxyl-terminated waterborne polyurethane and 16 g of cationic modified graphene into a container, stir for 4 h, add 7.2 g of defoamer RhodoLine DF 6002, 9.7 g of dispersant BYK-2013, and 120 g of waterborne bright red slurry, stir and disperse, and finally add 210 g of polymethylene polyphenyl isocyanate to obtain a wear-resistant modified waterborne polyurethane floor mortar coating.

[0048] Comparative Example 1

[0049] (1) Add 1000 g of hydroxyl-terminated waterborne polyurethane (prepared according to the method of Example 1), 7.2 g of defoamer RhodoLine DF 6002, 9.7 g of dispersant BYK-2013, and 120 g of waterborne bright red slurry into a container, stir and disperse, and finally add 210 g of polymethylene polyphenyl isocyanate to obtain a wear-resistant modified waterborne polyurethane floor mortar coating.

[0050] Comparative Example 2

[0051] (1) Add 1000 g of hydroxyl-terminated waterborne polyurethane (prepared according to the method of Example 1) and 2 g of graphene oxide into a container, stir for 2 h, add 7.2 g of defoamer RhodoLine DF 6002, 9.7 g of dispersant BYK-2013, and 120 g of waterborne bright red slurry, stir and disperse, and finally add 210 g of polymethylene polyphenyl isocyanate to obtain a wear-resistant modified waterborne polyurethane floor mortar coating.

[0052] Comparative Example 3

[0053] (1) Add dried polyester polyol 2000 with a hydroxyl content of 260 mmol and 110 mmol sodium 1,2-dihydroxy-3-propanesulfonate into the reactor. 50mL of N,N-dimethylformamide solvent was introduced with nitrogen, heated to 80°C, 100mmol of hexamethylene diisocyanate and 0.9mmol of dibutyltin dilaurate were added, and the reaction was carried out for 3h. The N,N-dimethylformamide solvent was removed by vacuum distillation, 800mL of water was added, and the mixture was stirred and dispersed to obtain a hydroxy-terminated waterborne polyurethane.

[0054] (2) Add 1000 g of hydroxyl-terminated waterborne polyurethane and 2 g of cationic modified graphene into a container, stir for 2 h, add 7.2 g of defoamer RhodoLine DF 6002, 9.7 g of dispersant BYK-2013, and 120 g of waterborne bright red slurry, stir and disperse, and finally add 210 g of polymethylene polyphenyl isocyanate to obtain a wear-resistant modified waterborne polyurethane floor mortar coating.

[0055] Pour the wear-resistant modified waterborne polyurethane floor mortar coating on the surface of the substrate, cure it at 50°C for 12 hours, and cure it at room temperature for 7 days to form a paint film. The flexibility of the paint film is tested according to GB / T 1731-2020 standard.

[0056] Staphylococcus aureus and Escherichia coli were cultured and activated and diluted to a concentration of 10 7 cfu / mL of bacterial suspension; 0.5mL of bacterial suspension was coated on the surface of the paint film, and the polyurethane floor mortar paint film of comparative example 1 was used as a blank control group. Then it was covered with a sterilized polyethylene film, placed in an incubator, and cultured at 37°C for 24 hours, and the bacteria on the surface of the paint film and the polyethylene film were eluted with a physiological saline eluent; then 0.2mL of the eluent was transferred and coated on the surface of the beef extract peptone agar culture medium, placed in an incubator, and cultured at 37°C for 24 hours; after culture, the live bacteria were counted; and the antibacterial rate R was calculated.

[0057] R = (BC) / B × 100%. B is the average number of recovered bacteria in the blank control group. C is the average number of recovered bacteria in the experimental group.

[0058] The wear-resistant modified waterborne polyurethane floor mortar coating was cured to form a film sample. The Shore hardness was tested according to GB / T 2411-2008 standard.

[0059] The friction test was conducted using a wear tester with a load of 19.6N, a rotation speed of 200r / min, and a test time of 60min. The wear amount per unit area R was calculated. R = △m / (L×d). △m is the mass loss of the film sample before and after friction. L is the width of the film sample, and d is the width of the wear scar.

[0060] Table 1 Paint film performance test

[0061]

[0062] As shown in Table 1, compared with Comparative Example 1, each embodiment adds cation-modified graphene, and graphene is better in dispersibility after surface organic modification, is not easy to agglomerate in waterborne polyurethane coating, and graphene surface contains a large amount of cationic quaternary ammonium salt groups, can be very strong bactericidal performance, can improve the antibacterial performance of polyurethane coating. At the same time, the cationic quaternary ammonium salt on the graphene surface can electrostatically interact with the sodium sulfonate anion in the polyurethane molecular chain, further enhance the interfacial bonding strength between graphene and polyurethane, make graphene play excellent reinforcing effect, significantly improve the hardness of coating paint film, reduce unit area wear amount, improve wear resistance. And polyphenyl sodium sulfonate chain extender contains a large amount of rigid benzene rings, is introduced into the polyurethane molecular chain, is conducive to improving the hardness and wear resistance of polyurethane.

[0063] Compared with Example 1, Comparative Example 2 adds unmodified graphene oxide, which has poor dispersibility, is easy to agglomerate, and cannot electrostatically interact with the sodium sulfonate anions in the polyurethane molecular chain. The interfacial bonding strength between the polyurethane and the graphene oxide is low, the reinforcement effect is poor, the paint film hardness is low, and the wear resistance is poor.

[0064] Compared with Example 1, Comparative Example 3 uses conventional 1,2-dihydroxy-3-propanesulfonic acid sodium as a chain extender and does not contain a rigid benzene ring, resulting in the hardness of the high polyurethane being lower than that of Example 1, the wear amount per unit area being higher than that of Example 1, and the wear resistance being poor.

[0065] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a wear-resistant modified waterborne polyurethane floor mortar coating, characterized in that: The preparation method is as follows: Step A, adding dry polyester polyol, sodium polyphenyl sulfonate chain extender, N,N-dimethylformamide solvent into a reaction kettle, introducing nitrogen, heating to 75-85° C., adding diisocyanate and dibutyltin dilaurate, reacting for 3-4 hours, removing N,N-dimethylformamide solvent by vacuum distillation, adding water, stirring and dispersing, and obtaining hydroxyl-terminated waterborne polyurethane; The sodium polyphenyl sulfonate chain extender has the structural formula (I) as follows: Step B, add hydroxyl-terminated waterborne polyurethane and cationically modified graphene into a container, stir for 2-4 hours, then add defoamer, dispersant, color paste, stir and disperse, and finally add polymethylene polyphenyl isocyanate to obtain wear-resistant modified waterborne polyurethane floor mortar coating.

2. The method for preparing the wear-resistant modified waterborne polyurethane floor mortar coating according to claim 1, characterized in that: In the step A, the molar ratio of the hydroxyl content of the polyester polyol, the sodium polyphenyl sulfonate chain extender, and the diisocyanate is (2.3-2.6):(1-1.2):1:(0.008-0.009).

3. The method for preparing the wear-resistant modified waterborne polyurethane floor mortar coating according to claim 2, characterized in that: The diisocyanate is hexamethylene diisocyanate, isophorone diisocyanate or toluene diisocyanate.

4. The method for preparing the wear-resistant modified waterborne polyurethane floor mortar coating according to claim 2, characterized in that: The preparation method of the sodium polyphenyl sulfonate chain extender comprises: adding toluene, 2,2'-sodium sulfonate-4,4'-diphenyl ether dicarboxylic acid, phenyl glycidyl ether and tetrabutylammonium bromide into a reaction bottle equipped with a condenser reflux tube, performing reduced pressure distillation, washing and recrystallization after the reaction to obtain the sodium polyphenyl sulfonate chain extender.

5. The method for preparing the wear-resistant modified waterborne polyurethane floor mortar coating according to claim 4, characterized in that: The molar ratio of the 2,2'-sodium sulfonate-4,4'-diphenyl ether dicarboxylic acid, phenyl glycidyl ether, and tetrabutylammonium bromide is 1:(2.2-2.6):(0.07-0.08).

6. The method for preparing the wear-resistant modified waterborne polyurethane floor mortar coating according to claim 4, characterized in that: The reaction temperature is 100-110° C. and the reaction time is 8-12 hours.

7. The method for preparing the wear-resistant modified waterborne polyurethane floor mortar coating according to claim 1, characterized in that: In the step B, the mass ratio of the hydroxyl-terminated waterborne polyurethane to the cation-modified graphene is 100:(0.2-2).

8. The method for preparing the wear-resistant modified waterborne polyurethane floor mortar coating according to claim 7, characterized in that: The preparation method of the cation-modified graphene is as follows: treating graphene oxide in thionyl chloride, dispersing the obtained chlorinated graphene in dichloromethane, adding 1,3-di(dodecyl quaternary ammonium salt) propanol and triethylamine, stirring at room temperature for reaction for 18-36 hours, filtering, washing, and drying to obtain the cation-modified graphene.

9. The method for preparing the wear-resistant modified waterborne polyurethane floor mortar coating according to claim 8, characterized in that: The mass ratio of the chlorinated graphene, 1,3-di(dodecyl quaternary ammonium salt) propanol, and triethylamine is 100:(200-600):(40-180).

10. Application of the wear-resistant modified waterborne polyurethane floor mortar coating obtained by the preparation method according to any one of claims 1 to 9 in floor mortar.

Citation Information

Cited By

  • Preparation method of two-component polyurethane anti-wear marking paint

    CN120310412A

  • Ceramic nozzle material and preparation method thereof

    CN120574034A