High and low temperature resistant anti-shrinkage glue, preparation method thereof and film coated PAM (Polyacrylamide) three-proofing board containing anti-shrinkage glue
By preparing a high-low temperature and anti-shrinkage rubber containing polyolefins, hydroxy polyacrylates and other components, the problem of existing waterproof coils and coated metal sheets being easily degummed and shrinked under high and low temperature environments is solved, and efficient The bonding and protection effect improves the weather resistance and wind resistance of the coated PAM three-protective plate.
Patent Information
- Application Number
- CN202411228086.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-26
AI Technical Summary
Existing waterproof coils and coated metal sheets are prone to degumming, shrinking and cracking in high and low temperatures and complex environments, resulting in protection failure. The commercially available anti-shrinkage anti-shrinkage performance is poor in high and low temperature resistance and is easy to peel.
A high and low temperature resistance anti-shrinkage glue is adopted, and its composition includes polyolefins, hydroxy polyacrylates, chlorine acetic resins, silicone modifiers, maleic anhydride grafted polyethylene and anti-aging agents, and is extruded by high-speed stirring and twin screws. The machine discharge process forms an adhesive layer for the preparation of coated PAM three-blocking plate.
It improves the adhesion between the coil and the metal plate, avoids the phenomenon of curling, enhances the protective performance and wind resistance of the composite material, extends the service life, and maintains waterproof and corrosion resistance in high and low temperature environments.
Smart Images

Figure BDA0005025261490000161 
Figure BDA0005025261490000171 
Figure BDA0005025261490000172
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials and construction engineering, and in particular to a high and low temperature resistant anti-shrinkage adhesive and a preparation method thereof, and a film-coated PAM three-proof board comprising the anti-shrinkage adhesive. Background Art
[0002] The metal roof of a building is a rigid structure, which mainly relies on anti-corrosion coating or self-waterproofing. Due to the poor self-waterproofing performance of the structure, natural environmental factors and operating conditions, the metal roof is prone to leakage. Due to the demand for metal roof systems for large-span steel structures, the construction environment is limited and a metal roof system with a short construction period is required. At the same time, during the maintenance or replacement stage of the metal roof system, it is urgent to replace the roof waterproofing products with high efficiency and long service life.
[0003] As a type of functional composite material product widely used in factories, transportation facilities, large buildings and other fields, waterproofing coils and coated metal sheets are gradually replacing outdoor protection and color-coated plates, and protecting buildings and materials. However, since these materials are directly exposed to the atmospheric environment, the weather resistance of waterproofing coils and coated metal sheets is reduced after being exposed to environmental factors such as solar radiation, rain and snow, temperature differences and strong winds. In particular, coated metal sheets are prone to degumming, shrinkage and cracking under the influence of complex environmental factors, because the thermal conductivity and expansion coefficient of each component material are significantly different, and the deformation capacity is different. This makes the protection ineffective and causes corrosion and leakage of metal parts. In addition, coated metal sheets are usually hot-pressed and then quickly cooled. The internal stress in the structural layer is large and released slowly, which can easily cause shrinkage after compounding.
[0004] There are some commercially available anti-shrinkage adhesives, but these anti-shrinkage adhesives have poor high and low temperature resistance and are easily peeled off from the substrate. Therefore, there is a need for an anti-shrinkage adhesive with excellent performance, especially high and low temperature resistance and not easy to peel off. Summary of the invention
[0005] In order to make up for the deficiencies of the prior art, the present invention provides a high and low temperature resistant anti-shrinkage adhesive and a preparation method thereof, and a film-coated PAM three-proof board comprising the anti-shrinkage adhesive.
[0006] In one aspect, the present invention provides a high and low temperature resistant anti-shrinkage adhesive, which comprises the following components in parts by weight:
[0007] Polyolefin 10-80 parts,
[0008] 0-5 parts of hydroxy polyacrylate,
[0009] Chlorovinyl resin 0-10 parts,
[0010] 0-5 parts of silicone modifier,
[0011] 2-20 parts of maleic anhydride grafted polyethylene, and
[0012] Anti-aging agent 0.2 to 2 parts.
[0013] Preferably, the high and low temperature resistant anti-shrinkage adhesive comprises the following components in parts by weight:
[0014] Polyolefin 40-80 parts,
[0015] 2-5 parts of hydroxy polyacrylate,
[0016] 5-10 parts of chloroacetic acid resin,
[0017] 2-5 parts of organic silicon modifier,
[0018] 2-8 parts of maleic anhydride grafted polyethylene, and
[0019] Anti-aging agent 0.2-1.2 parts.
[0020] More preferably, the high and low temperature resistant anti-shrinkage adhesive comprises the following components in parts by weight:
[0021] 60 parts of polyolefin,
[0022] 5 parts of hydroxy polyacrylate,
[0023] 10 parts of chloroacetic acid resin,
[0024] 5 parts of silicone modifier,
[0025] 4 parts of maleic anhydride grafted polyethylene, and
[0026] Anti-aging agent 0.9 parts.
[0027] Preferably, the polyolefin is selected from one or more of polyethylene, polypropylene, polyisobutylene, polystyrene, ethylene-propylene copolymer, ethylene-octene copolymer, ethylene-butene copolymer, ethylene-hexene copolymer, polystyrene-olefin copolymer and grafted polyolefins thereof.
[0028] More preferably, the polyolefin is a mixture of polyethylene, polypropylene, polyisobutylene and polystyrene-olefin copolymer.
[0029] Preferably, when the polyolefin is a mixture of polyethylene, polypropylene, polyisobutylene and polystyrene-olefin copolymer, the mass ratio between the polyethylene, the polypropylene, the polyisobutylene and the polystyrene-olefin copolymer is (0.5-2):(0.5-2):(6-10):(1-3), preferably 1:1:8:2.
[0030] Preferably, the polyolefin is a mixture of a medium molecular weight polyolefin and a high molecular weight polyolefin.
[0031] Preferably, the molecular weight of the medium molecular weight polyolefin (such as polyethylene, polypropylene, polyisobutylene and polystyrene-olefin copolymer) is 30,000 to 100,000, preferably 40,000 to 80,000.
[0032] Preferably, the molecular weight of the high molecular weight polyolefin (such as polyethylene, polypropylene, polyisobutylene and polystyrene-olefin copolymer) is 150,000 to 600,000, preferably 150,000 to 350,000.
[0033] Preferably, the mass ratio between the medium molecular weight polyolefin and the high molecular weight polyolefin is (0.5-2):(1-3), preferably 1.8:1.
[0034] Preferably, the hydroxy polyacrylate is selected from one or more of hydroxy poly methyl acrylate, hydroxy poly ethyl acrylate, hydroxy poly butyl acrylate, hydroxy poly (2-methacrylate) methyl ester, hydroxy poly (2-methacrylate) ethyl ester, and hydroxy poly (2-methacrylate) butyl ester.
[0035] More preferably, the hydroxypolyacrylate is selected from hydroxypolymethyl acrylate, hydroxypoly(2-methacrylate)methyl ester, hydroxypoly(2-methacrylate)ethyl ester.
[0036] Preferably, the molecular weight of the hydroxy polyacrylate is 30,000 to 200,000.
[0037] More preferably, the molecular weight of the hydroxy polyacrylate is 80,000 to 160,000.
[0038] Preferably, the chlorovinyl resin is selected from one or more of vinyl chloride acrylic acid copolymer resin and hydroxy vinyl chloride acrylic acid copolymer resin.
[0039] Preferably, the molecular weight of the chlorovinyl resin is 50,000 to 200,000.
[0040] More preferably, the molecular weight of the chlorovinyl resin is 60,000 to 120,000.
[0041] Preferably, the organosilicon modifier is selected from one or more of tetramethoxysilane, tetraethoxysilane and tetrabutoxysilane.
[0042] More preferably, the organosilicon modifier is tetraethoxysilane.
[0043] Preferably, the maleic anhydride grafted polyethylene is selected from at least one maleic anhydride grafted polyethylene having a maleic anhydride grafting rate of 1 to 10%.
[0044] More preferably, the maleic anhydride grafted polyethylene is selected from maleic anhydride grafted polyethylene with a maleic anhydride grafting rate of 3 to 6%.
[0045] Preferably, the molecular weight of the maleic anhydride grafted polyethylene is 30,000 to 200,000.
[0046] More preferably, the molecular weight of the maleic anhydride grafted polyethylene is 40,000 to 90,000.
[0047] Preferably, the anti-aging agent is selected from one or more of an antioxidant, an ultraviolet absorber and a light stabilizer.
[0048] Preferably, the high and low temperature resistant anti-shrinkage adhesive further comprises a dispersant and a plasticizer.
[0049] Preferably, the dispersant is selected from dispersants BK1142 and BK9076; preferably BK1142.
[0050] Preferably, the plasticizer is selected from di(2-ethylhexyl) phthalate, ethyl azelaate, dioctyl phthalate, preferably di(2-ethylhexyl) phthalate.
[0051] On the other hand, the present invention provides a method for preparing the above-mentioned high and low temperature resistant anti-shrinkage adhesive, which comprises the following steps: adding corresponding weight portions of polyolefin, hydroxy polyacrylate, chloroacetic acid resin, silicone modifier, maleic anhydride grafted polyethylene and anti-aging agent into a high-speed mixer according to the formula, stirring for 20-30 minutes to form a mixture, and then adding the mixture into a twin-screw extruder for melt blending, and extruding the mixture through the twin-screw extruder to obtain the mixture.
[0052] Furthermore, if the product is extruded by a twin-screw extruder and then cast by a casting roller, flattened and cooled by a guide roller, and rolled up after trimming, the high and low temperature resistant anti-shrinkage adhesive of the present invention is obtained.
[0053] The high and low temperature resistant shrinkage-proof adhesive of the present invention can be sold as a separate product. When sold, the shrinkage adhesive can be coated with a dustproof film on both sides. In a specific embodiment, it can be as follows Figure 1 As shown, dustproof films 1 and 3 are provided on both sides of the high and low temperature resistant anti-shrinkage adhesive (heat resistant anti-shrinkage adhesive) 2 of the present invention.
[0054] On the other hand, the present invention provides a PAM three-proof board, which can be divided into a single-sided PAM three-proof board and a double-sided PAM three-proof board, which includes a high and low temperature resistant anti-shrinkage adhesive layer, and the high and low temperature resistant anti-shrinkage adhesive layer is a layer formed by the above-mentioned high and low temperature resistant anti-shrinkage adhesive.
[0055] Preferably, the single-sided coated PAM three-proof board includes a high and low temperature resistant anti-shrinkage adhesive layer.
[0056] Preferably, the double-sided coated PAM three-proof board includes two layers of high and low temperature resistant anti-shrinkage adhesive layers.
[0057] Preferably, the coated PAM three-proof board is composed of at least one metal plate, at least one coiled material layer, and at least one high and low temperature resistant anti-shrinkage adhesive layer arranged between the at least one metal plate and the at least one coiled material layer, and the high and low temperature resistant anti-shrinkage adhesive layer is a layer formed by the high and low temperature resistant anti-shrinkage adhesive. The high and low temperature resistant anti-shrinkage adhesive of the present invention realizes the bonding and compounding of the coiled material layer and the metal plate.
[0058] Preferably, the metal plates include: aluminum and aluminum alloy plates, steel plates, stainless steel plates and copper plates.
[0059] More preferably, the metal plate includes: a galvanized steel plate, a galvanized aluminum steel plate, and an aluminum-manganese alloy plate.
[0060] Preferably, the coiled material layer is a waterproof material, including any one of a TPO coiled material, a PVC coiled material, a SBS coiled material and a PTFE coiled material.
[0061] Preferably, the thickness of the high and low temperature resistant anti-shrinkage adhesive layer is 0.05-0.5 mm;
[0062] More preferably, the thickness of the high and low temperature resistant anti-shrinkage adhesive layer is 0.1-0.3 mm.
[0063] Preferably, the thickness of the metal plate is 0.2-2 mm;
[0064] More preferably, the metal plate has a thickness of 0.8-1.6 mm.
[0065] Preferably, the thickness of the coiled material layer is 0.1-2 mm;
[0066] More preferably, the thickness of the coiled material layer is 0.2-1.5 mm.
[0067] In a specific embodiment, the film-coated PAM three-proof board is a single-sided film-coated PAM three-proof board, such as Figure 2 As shown, it includes a coiled material layer 4, a metal plate 6 and a heat-resistant and shrink-proof adhesive layer 5 arranged between the coiled material layer 4 and the metal plate 6. Optionally, it also includes a passivation anti-corrosion layer 7 arranged on the bottom surface of the metal plate 6.
[0068] In a specific embodiment, the film-coated PAM three-proof board is a double-sided film-coated PAM three-proof board, such as Figure 3 As shown, it includes a coiled material layer 8, a coiled material layer 12, a metal plate 10, and a heat-resistant and shrink-proof adhesive layer 11 arranged between the coiled material layers 8, 12 and the metal plate 10.
[0069] In one embodiment, the film-coated PAM three-proof board is prepared by the following steps:
[0070] Board type 1: Preparation of single-sided coated PAM three-proof board
[0071] First, the metal plate is spray-cleaned with a degreasing agent to clean the oil and dust on the surface of the substrate; the metal plate after surface treatment is coated with anti-corrosion and passivation treatment. Then, the treated metal plate is heated in an oven to a plate temperature of 160-220°C, and then matured and pressed in the laminating machine in the order of the top layer being the coil layer, the second top layer being the high and low temperature resistant anti-shrinkage adhesive layer, and the bottom layer being the metal plate. After the pressing is completed, it is cooled. Finally, the cooled single-sided laminated PAM three-proof board is rolled up to become a finished product.
[0072] Board type 2: Preparation of double-sided coated PAM three-proof board
[0073] First, the metal plate is spray-cleaned with a degreasing agent to clean the oil and dust on the surface of the substrate; the surface-treated metal plate is coated with anti-corrosion and passivation. Then, the treated metal plate is heated in an oven to a plate temperature of 160-220°C, and then matured and pressed in the order of the outermost layer on both sides of the metal plate as the coil layer, the secondary layer on both sides of the metal plate as the high and low temperature resistant anti-shrinkage adhesive layer, and the metal plate in the middle. After the pressing is completed, it is cooled. Finally, the double-sided laminated PAM three-proof board that has been cooled is rolled up to become a finished product.
[0074] The high and low temperature resistant anti-shrinkage adhesive of the present invention adopts solvent-free mixing and processing, which not only avoids the environmental pollution and safety hazards caused by solvents such as benzene, toluene and xylene during use; at the same time, the adhesive can withstand high and low temperatures, has good flowability after hot melting, and can avoid the shrinkage phenomenon of the coated metal sheet after hot pressing and compounding. In addition, the high and low temperature resistant anti-shrinkage adhesive has improved adhesion with metal plates and waterproof coils of different materials, and enhances the tightness of each structural layer of the composite material, thereby further improving the protective performance of the material in high and low temperature environments and the wind resistance under high wind speeds. Furthermore, during the use of the above-mentioned coated PAM three-proof board, the construction is more convenient and has excellent decorative and functional properties. Furthermore, the present invention also provides a technology for preparing a coated PAM three-proof board, which is conducive to realizing the expansion of the industrialization and large-scale new applications of metal plate and coil composite materials.
[0075] Compared with the prior art, the high and low temperature resistant anti-shrinkage adhesive and its coated PAM three-proof board of the present invention have excellent physical and chemical properties such as resistance to high and low temperature changes, waterproof, corrosion resistance, wind resistance, long-term weather resistance and flame retardancy; at the same time, they have high mechanical strength, resistance to bending, puncture, tearing and shrinkage, etc. At the same time, the waterproof coiled material and high and low temperature resistant anti-shrinkage adhesive included in the coiled material layer of the present invention are well combined with various metal plates, and will not debond or debond in complex environments such as vibration, alternating hot and cold, strong winds, and solar radiation. This product is environmentally friendly and safe during use, the product construction is convenient, and it has excellent decorative and protective properties. It has huge development potential and can be widely used in the protection of building roofs. BRIEF DESCRIPTION OF THE DRAWINGS
[0076] The present invention will be further described below in conjunction with the accompanying drawings.
[0077] Figure 1 This is a cross-sectional view of a high and low temperature resistant anti-shrinkage adhesive product;
[0078] Figure 2 This is a cross-sectional view of a single-sided coated PAM three-proof board;
[0079] Figure 3 This is a cross-sectional view of a double-sided coated PAM three-proof board;
[0080] In the figure, 1-dustproof film layer, 2-high and low temperature resistant anti-shrinkage adhesive layer (heat resistant anti-shrinkage adhesive layer), 3-dustproof film layer, 4-roll material layer, 5-high and low temperature resistant anti-shrinkage adhesive layer (heat resistant anti-shrinkage adhesive layer), 6-metal plate layer, 7-passivation anti-corrosion layer, 8-roll material layer, 9-high and low temperature resistant anti-shrinkage adhesive layer (heat resistant anti-shrinkage adhesive layer), 10-metal plate layer, 11-high and low temperature resistant anti-shrinkage adhesive layer (heat resistant anti-shrinkage adhesive layer), 12-roll material layer. DETAILED DESCRIPTION
[0081] The following embodiments are provided for a better understanding of the present invention, but are not limited to the best mode of implementation, and do not limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0082] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the prior art can be used. The reagents and other instruments used without specifying the manufacturer are all conventional reagent products that can be obtained commercially. Among them, the purchase of some raw materials is as follows, and the raw materials used unless otherwise specified are as follows:
[0083] Polystyrene-olefin copolymer: molecular weight 40,000-80,000, China Petrochemical Corporation;
[0084] Polyethylene: molecular weight is 180,000 to 280,000, China Petrochemical Corporation;
[0085] Polypropylene: molecular weight is 220,000 to 350,000, China Petrochemical Corporation;
[0086] Polyisobutylene: molecular weight 150,000 to 260,000, China Petrochemical Corporation;
[0087] Hydroxylated polymethyl acrylate: molecular weight 80,000 to 120,000, Beijing Qianmen Chemical Raw Materials Co., Ltd.
[0088] Hydroxylated poly(2-methacrylate) methyl ester: molecular weight 120,000-140,000, Beijing Qianmen Chemical Raw Materials Co., Ltd.
[0089] Hydroxylated poly(2-methacrylate) ethyl ester: molecular weight 130,000-160,000, Beijing Qianmen Chemical Raw Materials Co., Ltd.
[0090] Vinyl chloride acrylic acid copolymer resin: molecular weight 60,000 to 90,000, Hanwha Corporation;
[0091] Hydroxyvinyl chloride acrylic acid copolymer resin: molecular weight 80,000 to 120,000, from Wacker, Germany;
[0092] Tetramethoxysilane, tetraethoxysilane, tetrabutoxysilane: Beijing Qianmen Chemical Raw Materials Co., Ltd.;
[0093] Maleic anhydride grafted polyolefin resin: grafting rate is 4-6%, molecular weight is 40,000-90,000, Dow Chemical Company, USA;
[0094] Dispersant BK1142, light stabilizer BYK4371: BYK;
[0095] Di(2-ethylhexyl) phthalate, ethyl azelaate, diphenyl octyl phosphate: Beijing Qianmen Chemical Raw Materials Co., Ltd.;
[0096] Antioxidant 1010: Nanjing Huali Mingke Industry and Trade Co., Ltd.;
[0097] Ultraviolet absorber UV-327: Nanjing Huali Mingke Industry and Trade Co., Ltd.;
[0098] TPO roll, PVC roll: thickness 0.6~1.5mm, in line with the requirements of GB 27789-2011, commercially available;
[0099] Galvanized steel plate, galvanized aluminum steel plate, aluminum-manganese alloy plate: thickness 0.8~1.6mm, in line with the requirements of standard GB / T 3880.2-2012, commercially available.
[0100] Unless otherwise specified in the following examples, all parts are by weight.
[0101] The detection methods involved in the following test examples 1 to 4 are as follows:
[0102] The following testing method was used to test the main properties of the high and low temperature resistant anti-shrinkage adhesives of Examples 1-4 and Comparative Examples 1-4.
[0103] Adhesion (grade): GB / T 9286-2021 "Scratch test for paints and varnishes"
[0104] Peel strength: GB / T 2790-1995 "180° peel strength test method for adhesives - flexible materials to rigid materials"
[0105] Impact resistance: GB / T 1732-2020 "Determination of impact resistance of paint films"
[0106] Freeze-thaw resistance: GB / T 17748-2016 "Aluminum-plastic composite panels for building curtain walls" 7.7.4
[0107] Neutral salt spray test (salt spray corrosion resistance test): GB / T 10125-2021;
[0108] Resistance to artificial climate accelerated aging (ultraviolet): GB / T 16422.2-2014
[0109] Examples 1 to 8 Preparation of a high and low temperature resistant anti-shrinkage adhesive
[0110] Example 1 Preparation of high and low temperature resistant anti-shrinkage adhesive
[0111] Add 60 parts of polyolefin, including 5 parts of polyethylene, 5 parts of polypropylene, 40 parts of polyisobutylene, 10 parts of styrene-olefin copolymer, 5 parts of hydroxy poly(2-methacrylate) methyl ester, 10 parts of vinyl chloride acrylic acid copolymer resin, 5 parts of tetraethoxysilane, 4 parts of maleic anhydride grafted polyethylene, 1 part of dispersant, 1 part of plasticizer, 0.2 parts of antioxidant, 0.5 parts of ultraviolet absorber and 0.2 parts of light stabilizer into a high-speed mixer and stir for 20 to 30 minutes to form a mixture;
[0112] The mixed material is added into a twin-screw extruder for melt copolymerization, and extruded through the twin-screw extruder to form a high-temperature resistant and shrink-proof adhesive; the screw extrusion speed of the twin-screw extruder is 60-160 r / min, and the extrusion temperature is 120-160°C.
[0113] The high temperature resistant and anti-shrinkage adhesive particles are accurately metered by a metering pump, extruded from a mold at a temperature of 200-250°C, cast by a casting roller under the same temperature conditions, flattened and cooled by a guide roller, and accurately measured by a thickness gauge in the middle, trimmed, and then neatly rolled up by a traction and winder to finally make a high and low temperature resistant and anti-shrinkage adhesive film.
[0114] Example 2 Preparation of high and low temperature resistant anti-shrinkage adhesive
[0115] Add 60 parts of polyolefin, including 5 parts of polyethylene, 5 parts of polypropylene, 40 parts of polyisobutylene, 10 parts of styrene-olefin copolymer, 5 parts of hydroxy poly(2-methacrylate) methyl ester, 10 parts of hydroxy vinyl chloride acrylic copolymer resin, 5 parts of tetraethoxysilane, 4 parts of maleic anhydride grafted polyethylene, 1 part of dispersant, 1 part of plasticizer, 0.2 parts of antioxidant, 0.5 parts of ultraviolet absorber and 0.2 parts of light stabilizer into a high-speed mixer and stir for 20 to 30 minutes to form a mixture;
[0116] The mixed material is added into a twin-screw extruder for melt copolymerization, and extruded through the twin-screw extruder to form a high-temperature resistant and shrink-proof adhesive; the screw extrusion speed of the twin-screw extruder is 60-160 r / min, and the extrusion temperature is 120-160°C.
[0117] The high temperature resistant and anti-shrinkage adhesive particles are accurately metered by a metering pump, extruded from a mold at a temperature of 200-250°C, cast by a casting roller under the same temperature conditions, flattened and cooled by a guide roller, and accurately measured by a thickness gauge in the middle, trimmed, and then neatly rolled up by a traction and winder to finally make a high and low temperature resistant and anti-shrinkage adhesive film.
[0118] Example 3 Preparation of high and low temperature resistant anti-shrinkage adhesive
[0119] Add 60 parts of polyolefin, including 5 parts of polyethylene, 5 parts of polypropylene, 40 parts of polyisobutylene, 10 parts of styrene-olefin copolymer, 5 parts of hydroxy poly(2-methylacrylate), 10 parts of hydroxy vinyl chloride acrylic copolymer resin, 5 parts of tetraethoxysilane, 4 parts of maleic anhydride grafted polyethylene, 1 part of dispersant, 1 part of plasticizer, 0.2 parts of antioxidant, 0.5 parts of ultraviolet absorber and 0.2 parts of light stabilizer into a high-speed mixer and stir for 20 to 30 minutes to form a mixture;
[0120] The mixed material is added into a twin-screw extruder for melt copolymerization, and extruded through the twin-screw extruder to form a high-temperature resistant and shrink-proof adhesive; the screw extrusion speed of the twin-screw extruder is 60-160 r / min, and the extrusion temperature is 120-160°C.
[0121] The high temperature resistant and anti-shrinkage adhesive particles are accurately metered by a metering pump, extruded from a mold at a temperature of 200-250°C, cast by a casting roller under the same temperature conditions, flattened and cooled by a guide roller, and accurately measured by a thickness gauge in the middle, trimmed, and then neatly rolled up by a traction and winder to finally make a high and low temperature resistant and anti-shrinkage adhesive film.
[0122] Example 4 Preparation of high and low temperature resistant anti-shrinkage adhesive
[0123] Add 60 parts of polyolefin, including 5 parts of polyethylene, 5 parts of polypropylene, 40 parts of polyisobutylene, 10 parts of styrene-olefin copolymer, 5 parts of hydroxy polymethyl acrylate, 10 parts of hydroxy vinyl chloride acrylic copolymer resin, 5 parts of tetraethoxysilane, 4 parts of maleic anhydride grafted polyethylene, 1 part of dispersant, 1 part of plasticizer, 0.5 parts of antioxidant, 0.5 parts of ultraviolet absorber and 0.5 parts of light stabilizer into a high-speed mixer and stir for 20 to 30 minutes to form a mixture;
[0124] The mixed material is added into a twin-screw extruder for melt copolymerization, and extruded through the twin-screw extruder to form a high-temperature resistant and shrink-proof adhesive; the screw extrusion speed of the twin-screw extruder is 60-160 r / min, and the extrusion temperature is 120-160°C.
[0125] The high temperature resistant and anti-shrinkage adhesive particles are accurately metered by a metering pump, extruded from a mold at a temperature of 200-250°C, cast by a casting roller under the same temperature conditions, flattened and cooled by a guide roller, and accurately measured by a thickness gauge in the middle, trimmed, and then neatly rolled up by a traction and winder to finally make a high and low temperature resistant and anti-shrinkage adhesive film.
[0126] Example 5 Preparation of high and low temperature resistant anti-shrinkage adhesive
[0127] Add 20 parts of polyolefins, including 2 parts of polyethylene, 2 parts of polypropylene, 14 parts of polyisobutylene, 2 parts of styrene-olefin copolymer, 2 parts of hydroxy poly(2-methylacrylate) methyl ester, 1 part of vinyl chloride acrylic acid copolymer resin, 2 parts of tetraethoxysilane, 1 part of maleic anhydride grafted polyethylene, 0.2 parts of dispersant, 0.1 parts of plasticizer, 0.1 parts of antioxidant, 0.1 parts of ultraviolet absorber and 0.1 parts of light stabilizer into a high-speed mixer and stir for 20 to 30 minutes to form a mixture;
[0128] The mixed material is added into a twin-screw extruder for melt copolymerization, and extruded through the twin-screw extruder to form a high-temperature resistant and shrink-proof adhesive; the screw extrusion speed of the twin-screw extruder is 60-160 r / min, and the extrusion temperature is 120-160°C.
[0129] The high temperature resistant and anti-shrinkage adhesive particles are accurately metered by a metering pump, extruded from a mold at a temperature of 200-250°C, cast by a casting roller under the same temperature conditions, flattened and cooled by a guide roller, and accurately measured by a thickness gauge in the middle, trimmed, and then neatly rolled up by a traction and winder to finally make a high and low temperature resistant and anti-shrinkage adhesive film.
[0130] Example 6 Preparation of high and low temperature resistant anti-shrinkage adhesive
[0131] Add 40 parts of polyolefin, including 5 parts of polyethylene, 5 parts of polypropylene, 25 parts of polyisobutylene, 5 parts of styrene-olefin copolymer, 2 parts of hydroxy poly(2-methacrylate) methyl ester, 2 parts of vinyl chloride acrylic acid copolymer resin, 2 parts of tetraethoxysilane, 1 part of maleic anhydride grafted polyethylene, 0.2 parts of dispersant, 0.2 parts of plasticizer, 0.2 parts of antioxidant, 0.2 parts of ultraviolet absorber, and 0.2 parts of light stabilizer into a high-speed mixer, and stir for 20 to 30 minutes to form a mixture;
[0132] The mixed material is added into a twin-screw extruder for melt copolymerization, and extruded through the twin-screw extruder to form a high-temperature resistant and shrink-proof adhesive; the screw extrusion speed of the twin-screw extruder is 60-160 r / min, and the extrusion temperature is 120-160°C.
[0133] The high temperature resistant and anti-shrinkage adhesive particles are accurately metered by a metering pump, extruded from a mold at a temperature of 200-250°C, cast by a casting roller under the same temperature conditions, flattened and cooled by a guide roller, and accurately measured by a thickness gauge in the middle, trimmed, and then neatly rolled up by a traction and winder to finally make a high and low temperature resistant and anti-shrinkage adhesive film.
[0134] Example 7 Preparation of high and low temperature resistant anti-shrinkage adhesive
[0135] Add 40 parts of polyolefin, including 5 parts of polyethylene, 5 parts of polypropylene, 25 parts of polyisobutylene, 5 parts of styrene-olefin copolymer, 2 parts of hydroxy poly(2-methacrylate) methyl ester, 2 parts of hydroxy vinyl chloride acrylic copolymer resin, 2 parts of tetraethoxysilane, 1 part of maleic anhydride grafted polyethylene, 0.2 parts of dispersant, 0.1 parts of plasticizer, 0.1 parts of antioxidant, 0.1 parts of ultraviolet absorber and 0.1 parts of light stabilizer into a high-speed mixer and stir for 20 to 30 minutes to form a mixture;
[0136] The mixed material is added into a twin-screw extruder for melt copolymerization, and extruded through the twin-screw extruder to form a high-temperature resistant and shrink-proof adhesive; the screw extrusion speed of the twin-screw extruder is 60-160 r / min, and the extrusion temperature is 120-160°C.
[0137] The high temperature resistant and anti-shrinkage adhesive particles are accurately metered by a metering pump, extruded from a mold at a temperature of 200-250°C, cast by a casting roller under the same temperature conditions, flattened and cooled by a guide roller, and accurately measured by a thickness gauge in the middle, trimmed, and then neatly rolled up by a traction and winder to finally make a high and low temperature resistant and anti-shrinkage adhesive film.
[0138] Example 8 Preparation of high and low temperature resistant anti-shrinkage adhesive
[0139] Add 80 parts of polyolefin, including 5 parts of polyethylene, 5 parts of polypropylene, 25 parts of polyisobutylene, 5 parts of styrene-olefin copolymer, 2 parts of hydroxy poly(2-methacrylate) methyl ester, 10 parts of hydroxy vinyl chloride acrylic copolymer resin, 5 parts of tetraethoxysilane, 5 parts of maleic anhydride grafted polyethylene, 1.5 parts of dispersant, 0.5 parts of plasticizer, 0.5 parts of antioxidant, 1.0 parts of ultraviolet absorber and 1.0 parts of light stabilizer into a high-speed mixer and stir for 20 to 30 minutes to form a mixture;
[0140] The mixed material is added into a twin-screw extruder for melt copolymerization, and extruded through the twin-screw extruder to form a high-temperature resistant and shrink-proof adhesive; the screw extrusion speed of the twin-screw extruder is 60-160 r / min, and the extrusion temperature is 120-160°C.
[0141] The high temperature resistant and anti-shrinkage adhesive particles are accurately metered by a metering pump, extruded from a mold at a temperature of 200-250°C, cast by a casting roller under the same temperature conditions, flattened and cooled by a guide roller, and accurately measured by a thickness gauge in the middle, trimmed, and then neatly rolled up by a traction and winder to finally make a high and low temperature resistant and anti-shrinkage adhesive film.
[0142] Embodiments 9 to 17 Preparation of a TPO single-sided coated PAM three-proof board
[0143] Example 9 Preparation of a TPO single-sided coated PAM three-proof board
[0144] The galvanized steel plate (thickness 1.6mm) is sprayed with a degreasing agent to clean the oil and dust on the surface of the material, wherein the degreasing agent spray temperature is 40-60°C and the pressure is 0.4MPa; then chemical coating is carried out, and anti-corrosion treatment is performed on both sides of the metal plate. After coating, it is dried at 80-150°C to form a passivation coating with a dry film thickness of 5-10 microns. After the treated metal plate is heated in an oven to a plate temperature of 180-220°C, it is cured and pressed by a laminating machine in the order of the top layer being TPO coil (thickness 1.2mm), the second top layer being the high and low temperature resistant anti-shrinkage adhesive prepared in Example 1, and the metal plate in the middle, and then cooled after the pressing is completed. Finally, the metal-laminated plate that has been cooled is rolled up to obtain a TPO single-sided laminated PAM three-proof plate.
[0145] Example 10 Preparation of a TPO single-sided coated PAM three-proof board
[0146] The galvanized steel sheet (thickness 0.8mm) is sprayed with a degreasing agent to clean the oil and dust on the surface of the material, wherein the degreasing agent spray temperature is 40-60°C and the pressure is 0.4MPa; then chemical coating is carried out, and anti-corrosion treatment is performed on both sides of the metal plate. After coating, it is dried at 80-150°C to form a passivation coating with a dry film thickness of 5-10 microns. After the treated metal plate is heated in an oven to a plate temperature of 180-220°C, it is cured and pressed by a laminating machine in the order of the top layer being TPO coil (thickness 1.5mm), the second top layer being the high and low temperature resistant anti-shrinkage adhesive prepared in Example 1, and the metal plate in the middle, and then cooled after the pressing is completed. Finally, the metal-laminated plate that has been cooled is rolled up to obtain a TPO single-sided laminated PAM three-proof plate.
[0147] Embodiments 11 to 17 Preparation of a TPO single-sided coated PAM three-proof board
[0148] The material preparation processes of Examples 11 to 17 are similar to that of Example 10, except that the high and low temperature resistant anti-shrinkage adhesive used in the upper layer is replaced by the high and low temperature resistant anti-shrinkage adhesive prepared in Examples 2, 3, 4, 5, 6, 7 and 8, respectively, to finally obtain the TPO single-sided coated PAM three-proof panels of Examples 11 to 17.
[0149] Embodiments 18 to 21 Preparation of a TPO single-sided coated PAM three-proof board
[0150] The material preparation processes of Examples 18 to 21 are similar to those of Examples 9 and 10, except that the metal plates are replaced with galvanized aluminum steel plates (0.8 mm thick), galvanized aluminum steel plates (1.6 mm thick), aluminum-magnesium-manganese alloy plates (0.8 mm thick), and aluminum-magnesium-manganese alloy plates (1.2 mm thick), respectively, to finally obtain the TPO single-sided coated PAM three-proof plates of Examples 18 to 21.
[0151] Example 22 Preparation of a PVC single-sided coated PAM three-proof board
[0152] The galvanized steel plate (thickness 1.6mm) is sprayed with a degreasing agent to clean the oil and dust on the surface of the material, wherein the degreasing agent spray temperature is 40-60°C and the pressure is 0.4MPa; then chemical coating is carried out, and anti-corrosion treatment is performed on both sides of the metal plate. After coating, it is dried at 80-150°C to form a passivation coating with a dry film thickness of 5-10 microns. After the treated metal plate is heated in an oven to a plate temperature of 180-220°C, it is cured and pressed by a laminating machine in the order of the top layer being a PVC coil (thickness 1.2mm), the second top layer being the high and low temperature resistant anti-shrinkage film prepared in Example 1, and the metal plate in the middle, and then cooled after the pressing is completed. Finally, the metal-laminated plate that has been cooled is rolled up to obtain a PVC single-sided laminated PAM three-proof plate.
[0153] Example 23 Preparation of a PVC single-sided coated PAM three-proof board
[0154] The galvanized steel sheet (thickness 0.8mm) is sprayed with a degreasing agent to clean the oil and dust on the surface of the material, wherein the degreasing agent spray temperature is 40-60°C and the pressure is 0.4MPa; then chemical coating is carried out, and anti-corrosion treatment is performed on both sides of the metal plate. After coating, it is dried at 80-150°C to form a passivation coating with a dry film thickness of 5-10 microns. After the treated metal plate is heated in an oven to a plate temperature of 180-220°C, it is cured and pressed by a laminating machine in the order of the top layer being a PVC coil (thickness 1.5mm), the second top layer being the high and low temperature resistant anti-shrinkage film prepared in Example 1, and the metal plate in the middle, and then cooled after the pressing is completed. Finally, the metal-laminated plate that has been cooled is rolled up to obtain a PVC single-sided laminated PAM three-proof plate.
[0155] Example 24 Preparation of a TPO double-sided coated PAM three-proof board
[0156] The galvanized steel sheet (thickness 0.8mm) is sprayed with a degreasing agent to clean the oil and dust on the surface of the material, wherein the degreasing agent spray temperature is 40-60°C and the pressure is 0.4MPa; then chemical coating is carried out, and anti-corrosion treatment is performed on both sides of the metal plate. After coating, it is dried at 80-150°C to form a passivation coating with a dry film thickness of 5-10 microns. After the treated metal plate is heated in an oven to a plate temperature of 180-220°C, it is cured and pressed in the order of TPO coil (thickness 0.2mm) and TPO coil (thickness 1.5mm) on both sides of the metal plate, the second upper layers on both sides are the high and low temperature resistant anti-shrinkage film prepared in Example 1, and the metal plate in the middle, and then cooled after the pressing is completed. Finally, the metal coated plate that has been cooled is rolled up to obtain a TPO double-sided coated PAM three-proof plate.
[0157] Example 25 Preparation of a TPO double-sided coated PAM three-proof board
[0158] The galvanized steel sheet (thickness 1.2mm) is sprayed with a degreasing agent to clean the oil and dust on the surface of the material, wherein the degreasing agent spray temperature is 40-60°C and the pressure is 0.4MPa; then chemical coating is carried out, and anti-corrosion treatment is performed on both sides of the metal plate. After coating, it is dried at 80-150°C to form a passivation coating with a dry film thickness of 5-10 microns. After the treated metal plate is heated in an oven to a plate temperature of 180-220°C, it is cured and pressed in the order of TPO coil (thickness 0.2mm) and TPO coil (thickness 1.5mm) on both sides of the metal plate, the second upper layers on both sides are the high and low temperature resistant anti-shrinkage film prepared in Example 1, and the metal plate in the middle, and then cooled after the pressing is completed. Finally, the metal coated plate that has been cooled is rolled up to obtain a TPO double-sided coated PAM three-proof plate.
[0159] Example 26 Preparation of a PVC double-sided coated PAM three-proof board
[0160] The galvanized steel plate (thickness 0.8mm) is sprayed with a degreasing agent to clean the oil and dust on the surface of the material, wherein the degreasing agent spray temperature is 40-60°C and the pressure is 0.4MPa; then chemical coating is carried out, and anti-corrosion treatment is performed on both sides of the metal plate. After coating, it is dried at 80-150°C to form a passivation coating with a dry film thickness of 5-10 microns. After the treated metal plate is heated in an oven to a plate temperature of 180-220°C, it is cured and pressed in the order of the top layer on both sides of the metal plate being PVC coil (thickness 0.8mm), the second top layers on both sides being the high and low temperature resistant anti-shrinkage adhesive film prepared in Example 1, and the metal plate in the middle, and then cooled after the pressing is completed. Finally, the metal-laminated plate that has been cooled is rolled up to obtain a PVC double-sided laminated PAM three-proof plate.
[0161] Example 27 Preparation of a PVC double-sided coated PAM three-proof board
[0162] The galvanized steel sheet (thickness 1.2mm) is sprayed with a degreasing agent to clean the oil and dust on the surface of the material, wherein the degreasing agent spray temperature is 40-60°C and the pressure is 0.4MPa; then chemical coating is carried out, and anti-corrosion treatment is performed on both sides of the metal plate. After coating, it is dried at 80-150°C to form a passivation coating with a dry film thickness of 5-10 microns. After the treated metal plate is heated in an oven to a plate temperature of 180-220°C, it is cured and pressed in the order of the top layers on both sides of the metal plate being PVC coil (thickness 0.2mm) and PVC coil (thickness 1.5mm), the second upper layers on both sides are the high and low temperature resistant anti-shrinkage adhesive film prepared in Example 1, and the metal plate in the middle, and then cooled after the pressing is completed. Finally, the metal coated plate that has been cooled is rolled up to obtain a PVC double-sided coated PAM three-proof plate.
[0163] Comparative Examples 1 to 4 Preparation of a high and low temperature resistant anti-shrinkage adhesive
[0164] Comparative Example 1 Preparation of a high and low temperature resistant anti-shrinkage adhesive
[0165] Add 60 parts of polyolefin, including 5 parts of polyethylene, 5 parts of polypropylene, 40 parts of polyisobutylene, 10 parts of styrene-olefin copolymer, 4 parts of maleic anhydride grafted polyethylene, 1 part of dispersant, 1 part of plasticizer, 0.5 parts of antioxidant, 0.2 parts of ultraviolet absorber and 0.2 parts of light stabilizer into a high-speed mixer and stir for 20 to 30 minutes to form a mixture;
[0166] The mixed material is added into a twin-screw extruder for melt copolymerization, and extruded through the twin-screw extruder to form a high-temperature resistant and shrink-proof adhesive; the screw extrusion speed of the twin-screw extruder is 60-160 r / min, and the extrusion temperature is 120-160°C.
[0167] The high temperature resistant and anti-shrinkage adhesive particles are accurately metered by a metering pump, extruded from a mold at a temperature of 200-250°C, cast by a casting roller under the same temperature conditions, flattened and cooled by a guide roller, and accurately measured by a thickness gauge in the middle, trimmed, and then neatly rolled up by a traction and winder to finally make a high and low temperature resistant and anti-shrinkage adhesive film.
[0168] Comparative Example 2 Preparation of a high and low temperature resistant anti-shrinkage adhesive
[0169] Add 60 parts of polyolefin, including 5 parts of polyethylene, 5 parts of polypropylene, 40 parts of polyisobutylene, 10 parts of styrene-olefin copolymer, 10 parts of hydroxyvinyl chloride acrylic copolymer resin, 5 parts of tetraethoxysilane, 4 parts of maleic anhydride grafted polyethylene, 1 part of dispersant, 1 part of plasticizer, 0.5 parts of antioxidant, 0.2 parts of ultraviolet absorber and 0.2 parts of light stabilizer into a high-speed mixer and stir for 20 to 30 minutes to form a mixture;
[0170] The mixed material is added into a twin-screw extruder for melt copolymerization, and extruded through the twin-screw extruder to form a high-temperature resistant and shrink-proof adhesive; the screw extrusion speed of the twin-screw extruder is 60-160 r / min, and the extrusion temperature is 120-160°C.
[0171] The high temperature resistant and anti-shrinkage adhesive particles are accurately metered by a metering pump, extruded from a mold at a temperature of 200-250°C, cast by a casting roller under the same temperature conditions, flattened and cooled by a guide roller, and accurately measured by a thickness gauge in the middle, trimmed, and then neatly rolled up by a traction and winder to finally make a high and low temperature resistant and anti-shrinkage adhesive film.
[0172] Comparative Example 3 Preparation of a high and low temperature resistant anti-shrinkage adhesive
[0173] Add 60 parts of polyolefin, including 5 parts of polyethylene, 5 parts of polypropylene, 40 parts of polyisobutylene, 10 parts of styrene-olefin copolymer, 5 parts of hydroxy polymethyl acrylate, 5 parts of tetraethoxysilane, 4 parts of maleic anhydride grafted polyethylene, 1 part of dispersant, 1 part of plasticizer, 0.5 parts of antioxidant, 0.2 parts of ultraviolet absorber and 0.2 parts of light stabilizer into a high-speed mixer and stir for 20 to 30 minutes to form a mixture;
[0174] The mixed material is added into a twin-screw extruder for melt copolymerization, and extruded through the twin-screw extruder to form a high-temperature resistant and shrink-proof adhesive; the screw extrusion speed of the twin-screw extruder is 60-160 r / min, and the extrusion temperature is 120-160°C.
[0175] The high temperature resistant and anti-shrinkage adhesive particles are accurately metered by a metering pump, extruded from a mold at a temperature of 200-250°C, cast by a casting roller under the same temperature conditions, flattened and cooled by a guide roller, and accurately measured by a thickness gauge in the middle, trimmed, and then neatly rolled up by a traction and winder to finally make a high and low temperature resistant and anti-shrinkage adhesive film.
[0176] Comparative Example 4 Preparation of a high and low temperature resistant anti-shrinkage adhesive
[0177] Add 60 parts of polyolefin, including 5 parts of polyethylene, 5 parts of polypropylene, 40 parts of polyisobutylene, 10 parts of styrene-olefin copolymer, 5 parts of tetraethoxysilane, 4 parts of maleic anhydride grafted polyethylene, 1 part of dispersant, 1 part of plasticizer, 0.5 parts of antioxidant, 0.2 parts of ultraviolet absorber and 0.2 parts of light stabilizer into a high-speed mixer and stir for 20 to 30 minutes to form a mixture;
[0178] The mixed material is added into a twin-screw extruder for melt copolymerization, and extruded through the twin-screw extruder to form a high-temperature resistant and shrink-proof adhesive; the screw extrusion speed of the twin-screw extruder is 60-160 r / min, and the extrusion temperature is 120-160°C.
[0179] The high temperature resistant and anti-shrinkage adhesive particles are accurately metered by a metering pump, extruded from a mold at a temperature of 200-250°C, cast by a casting roller under the same temperature conditions, flattened and cooled by a guide roller, and accurately measured by a thickness gauge in the middle, trimmed, and then neatly rolled up by a traction and winder to finally make a high and low temperature resistant and anti-shrinkage adhesive film.
[0180] Comparative Examples 5-8 Preparation of a single-sided coated PAM three-proof board
[0181] Comparative Example 5 Preparation of a TPO single-sided coated PAM three-proof board
[0182] The galvanized steel sheet (thickness 1.6mm) is sprayed with a degreasing agent to clean the oil and dust on the surface of the material, wherein the degreasing agent spray temperature is 40-60°C and the pressure is 0.4MPa; then chemical coating is carried out, and anti-corrosion treatment is performed on both sides of the metal plate. After coating, it is dried at 80-150°C to form a passivation coating with a dry film thickness of 5-10 microns. After the treated metal plate is heated in an oven to a plate temperature of 180-220°C, it is cured and pressed by a laminating machine in the order of the top layer being TPO coil (thickness 0.8mm), the second top layer being the high and low temperature resistant anti-shrinkage adhesive prepared in Comparative Example 1, and the metal plate in the middle, and then cooled after the pressing is completed. Finally, the metal laminated plate that has been cooled is rolled up to obtain a TPO single-sided laminated PAM three-proof plate.
[0183] Comparative Examples 6-8 Preparation of a TPO single-sided coated PAM three-proof board
[0184] The material preparation processes of Comparative Examples 6 to 8 are similar to those of Comparative Example 5, except that the high and low temperature resistant anti-shrinkage adhesive used in the upper layer is replaced by the high and low temperature resistant anti-shrinkage adhesive prepared in Comparative Examples 2, 3 and 4, respectively, to finally prepare the TPO single-sided coated PAM three-proof boards of Comparative Examples 6 to 8.
[0185] Comparative Example 9 Preparation of a PVC single-sided coated PAM three-proof board
[0186] The galvanized steel sheet (thickness 1.6mm) is sprayed with a degreasing agent to clean the oil and dust on the surface of the material, wherein the degreasing agent spray temperature is 40-60°C and the pressure is 0.4MPa; then chemical coating is carried out, and anti-corrosion treatment is performed on both sides of the metal plate. After coating, it is dried at 80-150°C to form a passivation coating with a dry film thickness of 5-10 microns. After the treated metal plate is heated in an oven to a plate temperature of 180-220°C, it is ripened and pressed in the laminating machine in the order of the top layer being PVC coil (thickness 0.8mm), the second top layer being the high and low temperature resistant anti-shrinkage film prepared in Comparative Example 1, and the metal plate in the middle, and then cooled after the pressing is completed. Finally, the metal laminated plate that has been cooled is rolled up to obtain a PVC single-sided laminated PAM three-proof plate.
[0187] Test Example 1: Determination of the main properties of a high and low temperature resistant anti-shrinkage adhesive in Examples 1-8 and Comparative Examples 1-4
[0188] Table 1 Main performance test results of high and low temperature resistant anti-shrinkage adhesive of Examples 1-8
[0189]
[0190] Table 2 Main performance test results of high and low temperature resistant anti-shrinkage adhesive of comparative examples 1-4
[0191]
[0192] Test Example 2: Determination of the main properties of a TPO single-sided coated PAM three-proof board in Example 9-21
[0193] Table 3 Main performance test results of a TPO single-sided coated PAM three-proof board in Examples 9-15
[0194]
[0195]
[0196] Table 4 Main performance test results of a TPO single-sided coated PAM three-proof board in Examples 16-21
[0197]
[0198]
[0199] Test Example 3: Determination of the main properties of a PVC single / double-sided and TPO double-sided coated PAM three-proof board in Example 22-27
[0200] Table 5 Main performance test results of PVC single / double-sided and TPO double-sided coated PAM three-proof board in Examples 22-27
[0201]
[0202]
[0203] Test Example 4: Comparative Example 5-9: Determination of the main properties of a single-sided coated PAM three-proof board
[0204] Table 6 Comparative Examples 5-9 Main performance test results of a single-sided coated PAM three-proof board
[0205]
[0206]
[0207] The above measurement results show that the high and low temperature resistant anti-shrinkage adhesive provided by the embodiment of the present invention has excellent bonding performance and high bonding strength with concrete, metal substrate and polymer coil. At the same time, the PAM three-proof board made of high and low temperature resistant anti-shrinkage adhesive, metal plate and waterproof coil has a peel strength of 3.0N / mm and above at -40℃ and 80℃, and the salt spray corrosion resistance time exceeds 5000h, and the artificial climate aging test time exceeds 10000h. From the test results, it can be seen that the PAM three-proof board of the present invention has excellent high and low temperature resistance, weather resistance, and waterproof and anti-corrosion properties.
[0208] For the method embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the order of the actions described, because according to the present invention, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and components involved are not necessarily required by the present invention.
[0209] The above is a detailed introduction to a high and low temperature resistant anti-shrinkage adhesive and a coated PAM three-proof board provided by the present invention. Specific examples are used in this article to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea; at the same time, for general technicians in this field, according to the idea of the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.
Claims
1. A high and low temperature resistant anti-shrinkage adhesive, comprising the following components in parts by weight: Polyolefin 10-80 parts, 0-5 parts of hydroxy polyacrylate, Chlorovinyl resin 0-10 parts, 0-5 parts of silicone modifier, 2-20 parts of maleic anhydride grafted polyethylene, and Anti-aging agent 0.2 to 2 parts.
2. The high and low temperature resistant anti-shrinkage adhesive according to claim 1, wherein: The high and low temperature resistant anti-shrinkage adhesive comprises the following components in parts by weight: Polyolefin 40-80 parts, 2-5 parts of hydroxy polyacrylate, 5-10 parts of chloroacetic acid resin, 2-5 parts of organic silicon modifier, 2-8 parts of maleic anhydride grafted polyethylene, and Anti-aging agent 0.2-1.2 parts; Preferably, the high and low temperature resistant anti-shrinkage adhesive comprises the following components in parts by weight: 60 parts of polyolefin, 5 parts of hydroxy polyacrylate, 10 parts of chloroacetic acid resin, 5 parts of silicone modifier, 4 parts of maleic anhydride grafted polyethylene, and Anti-aging agent 0.9 parts.
3. The high and low temperature resistant anti-shrinkage adhesive according to claim 1 or 2, wherein: The polyolefin is selected from one or more of polyethylene, polypropylene, polyisobutylene, polystyrene, ethylene-propylene copolymer, ethylene-octene copolymer, ethylene-butene copolymer, ethylene-hexene copolymer, polystyrene-olefin copolymer and grafted polyolefins thereof, More preferably, the polyolefin is a mixture of polyethylene, polypropylene, polyisobutylene and polystyrene-olefin copolymer; Preferably, when the polyolefin is a mixture of polyethylene, polypropylene, polyisobutylene and polystyrene-olefin copolymer, the mass ratio of the polyethylene, the polypropylene, the polyisobutylene and the polystyrene-olefin copolymer is (0.5-2): (0.5-2): (6-10): (1-3), preferably 1:1:8:2; Preferably, the polyolefin is a mixture of a medium molecular weight polyolefin and a high molecular weight polyolefin; Preferably, the molecular weight of the medium molecular weight polyolefin (such as polyethylene, polypropylene, polyisobutylene and polystyrene-olefin copolymer) is 30,000 to 100,000, preferably 40,000 to 80,000; Preferably, the molecular weight of the high molecular weight polyolefin (such as polyethylene, polypropylene, polyisobutylene and polystyrene-olefin copolymer) is 150,000 to 600,000, preferably 150,000 to 350,000; Preferably, the mass ratio between the medium molecular weight polyolefin and the high molecular weight polyolefin is (0.5-2):(1-3), preferably 1.8:
1.
4. The high and low temperature resistant anti-shrinkage adhesive according to any one of claims 1 to 3, wherein: The hydroxy polyacrylate is selected from one or more of hydroxy poly methyl acrylate, hydroxy poly ethyl acrylate, hydroxy poly butyl acrylate, hydroxy poly (2-methacrylate) methyl ester, hydroxy poly (2-methacrylate) ethyl ester, and hydroxy poly (2-methacrylate) butyl ester; More preferably, the hydroxy polyacrylate is selected from hydroxy poly methyl acrylate, hydroxy poly (2-methacrylate) methyl ester, hydroxy poly (2-methacrylate) ethyl ester; Preferably, the molecular weight of the hydroxy polyacrylate is 30,000 to 200,000; More preferably, the molecular weight of the hydroxy polyacrylate is 80,000 to 160,000.
5. The high and low temperature resistant anti-shrinkage adhesive according to any one of claims 1 to 4, wherein: The chlorovinyl resin is selected from one or more of vinyl chloride acrylic acid copolymer resin and hydroxy vinyl chloride acrylic acid copolymer resin; Preferably, the molecular weight of the chlorovinyl resin is 50,000 to 200,000; More preferably, the molecular weight of the chlorovinyl resin is 60,000 to 120,000.
6. The high and low temperature resistant anti-shrinkage adhesive according to any one of claims 1 to 5, wherein: The organosilicon modifier is selected from one or more of tetramethoxysilane, tetraethoxysilane and tetrabutoxysilane; Preferably, the organosilicon modifier is tetraethoxysilane.
7. The high and low temperature resistant anti-shrinkage adhesive according to any one of claims 1 to 6, wherein: The maleic anhydride grafted polyethylene is selected from at least one maleic anhydride grafted polyethylene having a maleic anhydride grafting rate of 1 to 10%; More preferably, the maleic anhydride grafted polyethylene is selected from maleic anhydride grafted polyethylene having a maleic anhydride grafting rate of 3 to 6%; Preferably, the molecular weight of the maleic anhydride grafted polyethylene is 30,000 to 200,000; More preferably, the molecular weight of the maleic anhydride grafted polyethylene is 40,000 to 90,000; Preferably, the anti-aging agent is selected from one or more of an antioxidant, an ultraviolet absorber and a light stabilizer; Preferably, the high and low temperature resistant anti-shrinkage adhesive further comprises a dispersant and a plasticizer; Preferably, the dispersant is selected from dispersants BK1142 and BK9076; preferably BK1142; Preferably, the plasticizer is selected from di(2-ethylhexyl) phthalate, ethyl azelaate, dioctyl phthalate, preferably di(2-ethylhexyl) phthalate.
8. A method for preparing the high and low temperature resistant anti-shrinkage adhesive according to any one of claims 1 to 7, the method comprising the following steps: adding corresponding weight portions of polyolefin, hydroxy polyacrylate, chloroacetic acid resin, silicone modifier, maleic anhydride grafted polyethylene and anti-aging agent into a high-speed mixer according to the formula, stirring for 20-30 minutes to form a mixture, then adding the mixture into a twin-screw extruder for melt blending, and extruding through the twin-screw extruder to obtain the mixture.
9. A film-coated PAM three-proof board, divided into a single-sided film-coated PAM three-proof board and a double-sided film-coated PAM three-proof board, which includes a high and low temperature resistant anti-shrinkage adhesive layer, wherein the high and low temperature resistant anti-shrinkage adhesive layer is a layer formed by the above-mentioned high and low temperature resistant anti-shrinkage adhesive; Preferably, the single-sided coated PAM three-proof board includes a high and low temperature resistant anti-shrinkage adhesive layer; Preferably, the double-sided coated PAM three-proof board includes two layers of high and low temperature resistant anti-shrinkage adhesive layers; Preferably, the film-coated PAM three-proof board is composed of at least one metal plate, at least one coiled material layer, and at least one high and low temperature resistant anti-shrinkage adhesive layer arranged between the at least one metal plate and the at least one coiled material layer, and the high and low temperature resistant anti-shrinkage adhesive layer is a layer formed by the above-mentioned high and low temperature resistant anti-shrinkage adhesive; Preferably, the metal plate includes: aluminum and aluminum alloy plate, steel plate, stainless steel plate and copper plate; More preferably, the metal plate includes: galvanized steel plate, galvanized aluminum steel plate, aluminum-manganese alloy plate; Preferably, the coiled material layer is a waterproof material, including any one of a TPO coiled material, a PVC coiled material, a SBS coiled material and a PTFE coiled material.
10. The film-coated PAM three-proof board according to claim 9, wherein: The thickness of the high and low temperature resistant anti-shrinkage adhesive layer is 0.05-0.5mm; More preferably, the thickness of the high and low temperature resistant anti-shrinkage adhesive layer is 0.1-0.3 mm; Preferably, the thickness of the metal plate is 0.2-2 mm; More preferably, the thickness of the metal plate is 0.8-1.6 mm; Preferably, the thickness of the coiled material layer is 0.1-2 mm; More preferably, the thickness of the coiled material layer is 0.2-1.5 mm.