Adhesive and preparation method and application thereof
By using the bond produced by reacting epoxy resin with sulfide and polyol with isocyanate in non-pneumatic tires, the problem of insufficient bonding strength of the traditional bonding layer is solved, and rapid bonding and high bonding at low temperatures are achieved The effect of strength.
Patent Information
- Application Number
- CN202411105726.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Traditional polyurethane adhesives cannot meet the requirements of bonding strength during high-speed operation, emergency stop or emergency acceleration of non-pneumatic tires, resulting in lower bonding strength of the bonding layer.
Using a bond, including the first component and the second component, the bonding agent is formed with high adhesion and toughness by ring opening reaction of the epoxy resin with the sulfide and the prepolymer of the polyol with the isocyanate. A cement, used to bond the spokes to the tread.
It achieves rapid bonding at lower temperatures, improves bonding strength, meets the bonding requirements of non-pneumatic tires during high-speed operation and emergency stop or emergency acceleration, and has better performance.
Smart Images

Figure CN119019972A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of material technology, and in particular to an adhesive and a preparation method and application thereof. Background Art
[0002] With the development of technology, non-pneumatic tires, as tires for the new generation of electric vehicles, have been increasingly studied and applied. Non-pneumatic tires usually consist of three parts: tread, spokes, and hubs. The way these three parts fit together will affect the performance of the entire non-pneumatic tire.
[0003] Usually, a bonding layer is used to bond the spokes to the tread. Most of the rubbers that make up the tread are non-polar materials such as natural rubber, styrene-butadiene rubber, butadiene rubber and isoprene rubber, and the adhesive in the bonding layer is currently often polyurethane adhesives. However, if the spokes and the tread are bonded only with polyurethane adhesives containing isocyanate groups, the bonding strength is low and cannot meet the bonding strength requirements of the bonding layer of non-pneumatic tires during high-speed operation, sudden stop or sudden acceleration.
[0004] Therefore, it is urgent to develop a novel bonding layer for non-pneumatic tires to solve the above problems. Summary of the invention
[0005] The embodiments of the present application provide an adhesive and a preparation method and application thereof, thereby solving the problem that the traditional adhesive layer cannot achieve good bonding strength, resulting in the inability to meet the bonding strength requirements of the adhesive layer during high-speed operation, sudden stop or sudden acceleration of the non-pneumatic tire.
[0006] To achieve the above objectives, the embodiments of the present application adopt the following technical solutions:
[0007] In one aspect, a bonding material is provided, the bonding material comprising a first component and a second component;
[0008] The first component comprises by weight:
[0009] Epoxy resin, 30-50 parts;
[0010] Sulfide, 0.1-0.5 parts;
[0011] Accelerator, 0.1-1 part;
[0012] Catalyst, 0-0.1 parts;
[0013] Toughener, 3-5 parts;
[0014] Flame retardant, 3-5 parts;
[0015] The first solvent, 5-10 parts;
[0016] The second component comprises by weight:
[0017] Isocyanate, 30-40 parts;
[0018] Polyol, 1-10 parts;
[0019] Second solvent, 5-10 parts.
[0020] Furthermore, the ratio of the first component to the second component ranges from 100:10 to 100:15.
[0021] Further, the sulfide includes mercaptan;
[0022] The accelerator includes at least one of a tertiary amine accelerator and a pyridine accelerator;
[0023] The catalyst includes a metal catalyst;
[0024] The toughening agent includes a rubber toughening agent;
[0025] The flame retardant includes an organic phosphorus flame retardant;
[0026] The first solvent includes a ketone solvent.
[0027] Further, the polyol includes an alcohol containing multiple hydroxyl groups;
[0028] The second solvent includes a ketone solvent.
[0029] Further, the peel strength of the adhesive is in the range of 18-32 KN / m;
[0030] and / or,
[0031] The bonding temperature range of the adhesive is 1-25°C;
[0032] and / or,
[0033] The bonding time of the adhesive is in the range of 10-30 minutes.
[0034] On the other hand, an adhesive layer is provided, comprising the above adhesive.
[0035] In yet another aspect, a non-pneumatic tire is provided, comprising a spoke, a tread, and the above-mentioned bonding layer, wherein the bonding layer is used to bond the spoke to the tread.
[0036] On the other hand, a method for preparing the above-mentioned adhesive is provided, comprising the following steps:
[0037] obtaining the first component;
[0038] obtaining the second component;
[0039] The first component and the second component are mixed in a ratio of 100:10-100:15 to obtain the adhesive.
[0040] Further, obtaining the first component comprises:
[0041] Dehydrating the epoxy resin at 110-130° C. for 110-130 min to obtain a dehydrated epoxy resin;
[0042] After cooling the dehydrated epoxy resin to 50-70° C., the sulfide, the toughening agent, the flame retardant and the first solvent are added, and after uniform mixing, the accelerator and the catalyst are added. After reacting for a period of time, the first component is obtained.
[0043] Further, obtaining the second component comprises:
[0044] Dehydrating the polyol at 110-130° C. for 11-13 min to obtain a dehydrated polyol;
[0045] The dehydrated polyol is cooled to 30-50°C, and the second solvent is added to disperse the dehydrated polyol evenly. The isocyanate is then added to the dehydrated polyol in multiple times, and the reaction is continued for a period of time and the temperature is raised to 75-80°C. After further reaction for a period of time, the temperature is cooled to 25-30°C to obtain the second component.
[0046] The embodiments of the present application provide an adhesive and a preparation method and application thereof, wherein the epoxy groups in the epoxy resin and the thiol groups in the sulfide undergo a ring-opening reaction to generate molecules containing hydroxyl groups and a prepolymer of polyol-modified isocyanate obtained by the reaction of polyols with isocyanate groups. Then, the molecules containing hydroxyl groups can react with the prepolymer of polyol-modified isocyanate to obtain the adhesive of the embodiments of the present application. The adhesive has good adhesion, can be quickly bonded at a lower temperature, and has better performance.
[0047] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0049] Figure 1 A schematic diagram of the structure of a non-pneumatic tire provided in an embodiment of the present application;
[0050] Figure 2 A schematic diagram of a bonding layer and a tread provided in an embodiment of the present application;
[0051] Figure 3 A process flow chart of a preparation process of a bonding material provided in an embodiment of the present application;
[0052] Figure 4 A flow chart of another process for preparing an adhesive provided in an embodiment of the present application;
[0053] Figure 5 A process flow chart of another bonding material preparation method provided in an embodiment of the present application;
[0054] Figure 6 A flow chart of a preparation process of another adhesive provided in an embodiment of the present application. DETAILED DESCRIPTION
[0055] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0056] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0057] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or multiple, respectively.
[0058] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0059] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0060] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0061] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0062] In a first aspect, an embodiment of the present application provides an adhesive, which includes a first component and a second component.
[0063] The first component includes, by weight: 30-50 parts of epoxy resin; 0.1-0.5 parts of sulfide; 0.1-1 parts of accelerator; 0-0.1 parts of catalyst; 3-5 parts of toughening agent; 3-5 parts of flame retardant; and 5-10 parts of the first solvent.
[0064] The second component comprises, by weight: 30-40 parts of isocyanate; 1-10 parts of polyol; and 5-10 parts of a second solvent.
[0065] In practical applications, when the ratio of the first component to the second component is too high or too low, the strength of the bond is too low. Therefore, the ratio of the first component to the second component can be set in the range of 100:10-100:15, so that the strength of the bond can be better. Exemplarily, the ratio of the first component to the second component can be 100:10, 100:11, 100:12, 100:13, 100:14 or 100:15, etc.
[0066] It should be understood that the above epoxy resin has epoxy groups on its molecular chain.
[0067] In application, the sulfide may be thiol, etc. The thiol has a thiol (-SH) functional group on its molecular chain, that is, a thiol functional group, and the thiol here can be used as a curing agent.
[0068] The accelerator may be at least one of a tertiary amine accelerator and a pyridine accelerator, etc. The tertiary amine accelerator may include dimethylethanolamine, tetramethylethylenediamine, benzylxylene, N-methyl-N-hydroxyethyl-p-toluidine, triethanolamine, tripropylamine, etc.
[0069] It should be noted that the principle of pyridine accelerators is similar to that of tertiary amine accelerators, which will not be described in detail here.
[0070] Since the reactivity of thiols is very low, if a promoter is present, thiol ions can be formed to accelerate the reaction between the thiol group and the epoxy group. Based on the nucleophilic reaction mechanism, the epoxy groups in the epoxy resin and the thiol functional groups in the thiol can undergo a ring-opening reaction under the action of the promoter to generate molecules containing hydroxyl groups. The reaction is much faster and can be carried out at low temperatures.
[0071] The following is a reaction formula of epoxy resin and thiol:
[0072]
[0073] On the basis of the above, the amount of mercaptan can be controlled to obtain a high molecular weight modified epoxy resin. It should be noted that, first, the amount of mercaptan should not be too much to prevent curing. Second, the molecular weight of the modified epoxy resin is about twice or more than the molecular weight of the epoxy resin purchased on the market.
[0074] In the application, the catalyst may be a metal catalyst, for example, acetylacetone metal salt, and the metal ions in the acetylacetone metal salt may include iron ions (Fe 3+ ), cobalt ions (Co 3+ ), nickel ions (Ni 2+) or the like; or the catalyst may also be trioleate of tris(dimethylaminomethyl)phenol, etc. The catalyst here can promote the reaction between the epoxy group in the first component and the thiol group to produce a hydroxyl group, and the overall reaction rate can be controlled by controlling the amount of the catalyst.
[0075] The toughening agent may be a rubber toughening agent, such as nitrile rubber, etc. The toughening agent can be well dissolved in the first component by dissolving in the first solvent, and the toughening agent can be well dispersed in the epoxy resin during the gelation process, thereby improving the toughness of the epoxy resin.
[0076] The flame retardant may be an organic phosphorus flame retardant, such as triphosphate, etc. The organic phosphorus flame retardant contains a phosphoric acid group, can be finely dispersed in the first component system, and provides good flame retardant properties.
[0077] The first solvent may be a ketone solvent, such as butanone, etc. Adding a ketone solvent here is beneficial to the dispersion of other components in the first component and greatly reduces the viscosity of the mixed solution. In addition, it can also increase the uniformity of subsequent mixing with the second component, and effectively improve the dispersibility of the toughening agent and the flame retardant.
[0078] Exemplarily, the epoxy resin can be 30 parts, 35 parts, 40 parts, 45 parts, 48 parts or 50 parts by weight, etc.; the sulfide can be 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts or 0.5 parts by weight, etc.; the accelerator can be 0.1 parts, 0.2 parts, 0.4 parts, 0.6 parts, 0.8 parts or 1 parts by weight, etc.; the catalyst can be 0 parts, 0.02 parts, 0.04 parts, 0.06 parts, 0.08 parts or 0.1 parts by weight, etc.; the toughening agent can be 3 parts, 3.5 parts, 4 parts, 4.5 parts, 4.8 parts or 5 parts by weight, etc.; the flame retardant can be 3 parts, 3.5 parts, 4 parts, 4.5 parts, 4.8 parts or 5 parts by weight, etc.; the first solvent can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts by weight, etc.
[0079] In practical applications, the polyols may be alcohols containing two or more hydroxyl groups, such as polyester polyols, polymer polyols and polymeric polyols, and specifically may include ethylene glycol, propylene glycol, butylene glycol, glycerol, pentaerythritol, etc. The polyols here have a toughening effect in the molecule and can adjust the toughness. At the same time, the polyols can react with isocyanates to adjust the reactivity of the isocyanate groups. In addition, a mixture can be obtained after the polyols are modified, and the mixture includes a substance containing an isocyanate group at the end of a long molecular chain and a part of unreacted isocyanate, thereby adjusting the strength of the bond.
[0080] The second solvent may include a ketone solvent, such as butanone, etc. Adding a ketone solvent here is beneficial to the dispersion of other components in the second component and greatly reduces the viscosity of the mixed solution. In addition, it can also increase the uniformity of subsequent mixing with the first component, and effectively improve the dispersibility of the toughening agent and the flame retardant.
[0081] Exemplarily, the isocyanate can be 30 parts, 32 parts, 34 parts, 36 parts, 38 parts or 40 parts by weight, etc.; the polyol can be 1 part, 2 parts, 4 parts, 6 parts, 8 parts or 10 parts by weight, etc.; the second solvent can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts by weight, etc.
[0082] Thus, the second component is a prepolymer of polyol-modified isocyanate obtained by the reaction of isocyanate groups with hydroxyl groups in polyols. The prepolymer is a long-chain molecule terminated with isocyanate groups, and its structure is an alternating structural compound of polyols and isocyanates. The prepolymer can provide toughness to form the overall structure, reduce the activity of isocyanate, improve storage stability, and also increase the operating time when the first component and the second component are mixed.
[0083] Then, the embodiments of the present application can respectively generate a modified epoxy resin containing hydroxyl groups through a ring-opening reaction between the epoxy group in the epoxy resin and the thiol group in the sulfide, and a prepolymer of polyol-modified isocyanate obtained by the reaction of polyol and isocyanate group. Then, the modified epoxy resin containing hydroxyl groups can react with the prepolymer of polyol-modified isocyanate to obtain the adhesive of the embodiments of the present application.
[0084] In summary, the peel strength of the adhesive of the embodiment of the present application can range from 18 to 32 KN / m, which reflects the wide range and limit of the adhesive strength, that is, the adhesive has good adhesive strength. For example, the peel strength of the adhesive can be 18 KN / m, 20 KN / m, 24 KN / m, 27 KN / m, 30 KN / m or 32 KN / m, etc.
[0085] The bonding temperature range of the adhesive of the embodiment of the present application can be 1-25°C, which means that the adhesive can be bonded at a lower temperature. For example, the bonding temperature of the adhesive can be 1°C, 5°C, 10°C, 15°C, 18°C or 25°C.
[0086] The bonding time of the adhesive of the embodiment of the present application may range from 10 to 30 minutes, which means that the adhesive can be quickly bonded in a short time. For example, the bonding time of the adhesive may be 10 minutes, 15 minutes, 20 minutes, 25 minutes, 28 minutes or 30 minutes.
[0087] The embodiment of the present application provides an adhesive having good adhesion, and can be quickly bonded at a lower temperature, and has better performance.
[0088] In a second aspect, an embodiment of the present application provides an adhesive layer, comprising the above-mentioned adhesive.
[0089] The embodiment of the present application provides a bonding layer, which has good adhesion and can be quickly bonded at a lower temperature, thus having better performance.
[0090] In a third aspect, the present application provides a non-pneumatic tire, such as Figure 1 As shown, the non-pneumatic tire comprises a wheel spoke, a tread and the above-mentioned bonding layer, the wheel spoke comprises a plurality of spokes, and the bonding layer is arranged between the spoke and the tread and is used for bonding the spoke to the tread.
[0091] In addition, if Figure 1 As shown, the non-pneumatic tire may further include a hub, which is disposed on a side of the spokes away from the bonding layer and connected to a side of the spokes away from the bonding layer.
[0092] In applications, the material of the tread may include a rubber composition, and the raw rubber of the rubber composition may be selected from the group consisting of natural rubber, synthetic rubber, and a combination thereof.
[0093] Among them, the natural rubber can be conventional natural rubber or modified natural rubber. Conventional natural rubber can use any natural rubber as long as it is known as natural rubber, and the origin is not limited. For example, the natural rubber can contain cis-1,4-polyisoprene as the main agent, and can also contain trans-1,4-polyisoprene according to the required characteristics. Therefore, in addition to the natural rubber containing cis-1,4-polyisoprene as the main agent, the above-mentioned natural rubber can also contain trans-1,4-isoprene as the main agent.
[0094] Synthetic natural rubber refers to natural rubber obtained by modifying or purifying the above-mentioned conventional natural rubber, for example, epoxidized natural rubber (ENR), deproteinized natural rubber (DPNR), and hydrogenated natural rubber.
[0095] Figure 2 A schematic diagram of the structure after the bonding layer and the tread are combined in an embodiment of the present application is shown.
[0096] exist Figure 2In the figure, the solid line is epoxy resin, and the sphere is the cross-linking point structure, which is mainly the group generated by the reaction of hydroxyl groups generated by the ring-opening reaction between the epoxy groups in the epoxy resin and the thiol functional groups in the thiol with isocyanate, thereby forming an overall network structure. Therefore, the structure containing hydroxyl groups generated by the ring-opening reaction between the epoxy groups in the epoxy resin and the thiol functional groups in the thiol is bonded (or connected) by the group generated by the reaction of isocyanate and hydroxyl groups to form an adhesive; the dotted line is a rubber molecule, and the rubber molecule can be bonded by the adhesive.
[0097] The embodiment of the present application provides a non-pneumatic tire, in which the spokes and the tread can be bonded quickly and effectively via the bonding layer provided in the embodiment of the present application.
[0098] In a fourth aspect, an embodiment of the present application provides a method for preparing the above-mentioned adhesive.
[0099] like Figure 3 As shown, the preparation method of the adhesive comprises the following steps:
[0100] S1. Obtain a first component.
[0101] S2. Obtain a second component.
[0102] S3. Mix the first component and the second component in a ratio of 100:10-100:15 to obtain a bond.
[0103] For example, the ratio of the first component to the second component can be 100:10, 100:11, 100:12, 100:13, 100:14 or 100:15, etc.
[0104] Furthermore, if Figure 4 As shown, the above step S1, obtaining the first component includes:
[0105] S11, dehydrating the epoxy resin at 110-130° C. and 60-120 r / min for 110-130 min to obtain a dehydrated epoxy resin.
[0106] Since water reacts very quickly with isocyanate, water needs to be removed in advance to avoid consuming the groups involved in the reaction and to ensure the strength of the final bonding layer. However, since the water content of sulfides, toughening agents, and flame retardants is generally below 0.12%, it will not have any effect, so the epoxy resin is dehydrated in advance, and high-temperature dehydration is to prevent solvent volatilization.
[0107] For example, the dehydration temperature of the epoxy resin may be 110° C., 115° C., 120° C., 125° C., or 130° C., etc.
[0108] For example, the dehydration time of the epoxy resin may be 110 min, 115 min, 120 min, 125 min or 130 min, etc.
[0109] For example, the dehydration speed of the epoxy resin may be 60 r / min, 70 r / min, 80 r / min, 90 r / min, 110 r / min or 120 r / min, etc.
[0110] S12, after cooling the dehydrated epoxy resin to 50-70° C., add the sulfide, toughening agent, flame retardant and the first solvent, mix well and then add the accelerator and catalyst, react for 110-130 minutes to obtain the first component.
[0111] The purpose of cooling the dehydrated epoxy resin to 50-70° C. is to control the reaction rate, avoid explosion, and prevent the solvent from volatilizing in large quantities at high temperature.
[0112] For example, the temperature for cooling the dehydrated epoxy resin may be 50° C., 55° C., 60° C., 65° C., 68° C., or 70° C., etc.
[0113] For example, the reaction time may be 110 min, 115 min, 120 min, 125 min or 130 min, etc.
[0114] Furthermore, if Figure 5 As shown, the above step S2, obtaining the second component includes:
[0115] S21. Dehydrate the polyol at 110-130° C. and 80-100 r / min for 11-13 min to obtain dehydrated polyol.
[0116] Since water reacts with isocyanate very quickly, in order to avoid consuming the groups involved in the reaction and ensure the strength of the final bonding layer, the polyol is dehydrated in advance, and high-temperature dehydration is used to prevent solvent volatilization.
[0117] For example, the dehydration temperature of the polyol may be 110° C., 115° C., 120° C., 125° C., or 130° C., etc.
[0118] For example, the dehydration time of the polyol may be 11 min, 12 min, or 13 min, etc.
[0119] For example, the dehydration speed of the polyol may be 80 r / min, 85 r / min, 90 r / min, 95 r / min, 98 r / min or 100 r / min, etc.
[0120] S22, cooling the dehydrated polyol to 30-50°C, adding the second solvent to disperse evenly, adding isocyanate to the dehydrated polyol in multiple times, reacting for a period of time and heating to 75-80°C, and then reacting for a period of time, cooling to 25-30°C to obtain the second component.
[0121] In the application, the number of times of adding the isocyanate to the dehydrated polyol can be two, three, four, etc. Since adding the isocyanate once is prone to explosion and forms more low molecular weight substances, therefore, adding the isocyanate multiple times can control the deviation of the formed macromolecule in molecular weight distribution to be smaller.
[0122] For example, the temperature for cooling the dehydrated polyol may be 30° C., 35° C., 40° C., 45° C., 48° C., or 50° C., etc.
[0123] For example, isocyanate is added to the dehydrated polyol in multiple portions, and the temperature for reacting for a period of time and heating can be 75° C., 76° C., 77° C., 78° C., 79° C. or 80° C., etc.
[0124] For example, isocyanate is added to the dehydrated polyol in multiple portions, reacted for a period of time and heated to 75-80°C, and then reacted for a period of time, and then cooled to 25°C, 26°C, 27°C, 28°C, 29°C or 30°C.
[0125] Furthermore, if Figure 6 As shown, in the above step S22, the dehydrated polyol is cooled to 30-50°C, and then the isocyanate is added to the dehydrated polyol in multiple times, reacting for a period of time and heating to 75-80°C, and then reacting for a period of time, cooling to 25-30°C, and obtaining a second component comprising:
[0126] S221. Cool the dehydrated polyol to 30-50°C, add the second solvent and disperse it evenly, then add the isocyanate to the dehydrated polyol three times, react for 30 minutes each time for the first two times, react for 30 minutes after the third addition, heat to 75-80°C and react for 60 minutes, then cool to 25-30°C to obtain the second component.
[0127] An embodiment of the present application provides a method for preparing an adhesive, which first allows the epoxy group in the epoxy resin to undergo a ring-opening reaction with the thiol group in the sulfide to generate a molecule containing a hydroxyl group, and allows the polyol to react with the isocyanate group to generate a prepolymer of a polyol-modified isocyanate. Finally, the molecule containing the hydroxyl group reacts with the prepolymer of the polyol-modified isocyanate to generate an adhesive with good adhesion and can be quickly bonded at a lower temperature. In addition, the preparation method is simple, easy to implement, and low in cost.
[0128] The following is a specific preparation process of a non-pneumatic tire:
[0129] (1) Dehydrate the epoxy resin at 120°C and 60-120 r / min for 120 min to obtain a dehydrated epoxy resin.
[0130] (2) Cool the dehydrated epoxy resin to 50-70°C, add the sulfide, toughening agent, flame retardant and the first solvent to mix and disperse until the mixed liquid is uniform and has no stratification, then add a certain amount of accelerator and catalyst, and react at this temperature for 120 minutes to obtain the first component.
[0131] (3) Dehydrate the polyol at 120°C and 80-100 r / min for 12 min to obtain dehydrated polyol.
[0132] (4) Cool the dehydrated polyol to 30-50°C, add the second solvent and disperse evenly, then add the measured isocyanate in equal amounts to the polyol in three times, react for 30 minutes each time for the first two times, react for 30 minutes after the third addition, heat to 75-80°C and react for 60 minutes, then cool to 25-30°C to obtain the second component.
[0133] (5) Mix the first component and the second component in a ratio of 100:10-100:15 using a stirring device at 60-120 r / min for 2-5 minutes to obtain a bond.
[0134] (6) Blow the surface of each component of the non-pneumatic tire until there is no obvious floating or sinking matter on the surface.
[0135] (6) Use a coating device to apply or spray the adhesive to the locations where the parts need to be bonded.
[0136] (8) Assemble all components into one piece and place it under a pressure of 0.5-3MPa for more than 3 hours.
[0137] It should be noted that the description of the epoxy resin, sulfide, toughening agent, flame retardant, first solvent, polyol, isocyanate and second solvent in the embodiments of the present application can refer to the above embodiments and will not be repeated here.
[0138] The following uses a number of specific embodiments to illustrate the adhesives of the embodiments and comparative examples of the present application and their preparation methods and applications.
[0139] Example 1
[0140] (1) Dehydrate the epoxy resin at 120°C and 60 r / min for 120 min to obtain a dehydrated epoxy resin.
[0141] (2) The dehydrated epoxy resin was cooled to 50°C, and mercaptan, nitrile rubber, triphosphate and butanone were added to mix and disperse until the mixed solution was uniform and without stratification. A certain amount of N-methyl-N-hydroxyethyl-p-toluidine and ferric acetylacetonate were added, and the mixture was reacted at this temperature for 120 minutes to obtain the first component.
[0142] (3) Dehydrate the polyol at 120°C and 80 r / min for 12 min to obtain dehydrated polyol.
[0143] (4) Cool the dehydrated polyol to 30°C, add equal amounts of the measured isocyanate into the polyol in two portions, react for 30 minutes each time for the first addition, and react for 30 minutes after the second addition, heat to 75°C, react for 60 minutes, and then cool to 25°C to obtain the second component.
[0144] (5) Mix the first component and the second component in a ratio of 100:10 using a stirring device at 60 r / min for 2 minutes to obtain a bond.
[0145] Example 2
[0146] (1) Dehydrate the epoxy resin at 120°C and 100 r / min for 120 min to obtain a dehydrated epoxy resin.
[0147] (2) The dehydrated epoxy resin was cooled to 60°C, and mercaptan, nitrile rubber, triphosphate and butanone were added to mix and disperse until the mixed solution was uniform and without stratification. A certain amount of triethanolamine and cobalt acetylacetonate were added, and the mixture was reacted at this temperature for 120 minutes to obtain the first component.
[0148] (3) Dehydrate the polyol at 120°C and 90 r / min for 12 min to obtain dehydrated polyol.
[0149] (4) Cool the dehydrated polyol to 40°C, add equal amounts of the measured isocyanate into the polyol in three portions, react for 30 minutes each time for the first two times, react for 30 minutes after the third addition, heat to 78°C for 60 minutes, and then cool to 28°C to obtain the second component.
[0150] (5) The first component and the second component were mixed in a ratio of 100:13 using a stirring device at 100 r / min for 4 minutes to obtain a bond.
[0151] Example 3
[0152] (1) Dehydrate the epoxy resin at 120°C and 120 r / min for 120 min to obtain a dehydrated epoxy resin.
[0153] (2) The dehydrated epoxy resin was cooled to 70°C, and mercaptan, nitrile rubber, triphosphate and butanone were added to mix and disperse until the mixed solution was uniform and without stratification. A certain amount of tripropylamine and nickel acetylacetonate were added, and the mixture was reacted at this temperature for 120 minutes to obtain the first component.
[0154] (3) Dehydrate the polyol at 120°C and 100 r / min for 12 min to obtain dehydrated polyol.
[0155] (4) Cool the dehydrated polyol to 50°C, add equal amounts of the measured isocyanate into the polyol in four portions, react for 30 minutes each time for the first two times, and react for 30 minutes after the last two times, raise the temperature to 80°C and react for 60 minutes, then cool to 30°C to obtain the second component.
[0156] (5) Mix the first component and the second component in a ratio of 100:15 using a stirring device at 120 r / min for 5 minutes to obtain a bond.
[0157] Comparative Example 1
[0158] Commercially available polyurethane was used as the adhesive.
[0159] The peel strength of the adhesives obtained in Examples 1-3 and Comparative Example 1 was tested respectively, and the results are shown in Table 1 below.
[0160] According to GB / T 1524-2014 standard, the peel strength test was carried out in a tensile testing machine at a rate of 100 mm / min.
[0161] Table 1
[0162]
[0163] It can be seen from Table 1 that, compared with Comparative Example 1, the peel strengths of Examples 1-3 at 0.5 MPa, 1.5 MPa and 3.0 MPa are greater, and the bonding strengths of the adhesives prepared in Examples 1-3 are very good.
[0164] This application only introduces the contents related to the invention. The remaining structures can be obtained by referring to the relevant technologies and will not be described in detail here.
[0165] An “embodiment” referred to herein means that a particular feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment of the present application.
[0166] In the description provided herein, a large number of specific details are described. However, it is understood that the embodiments of the present application can be practiced without these specific details. In some instances, well-known methods, structures and techniques are not shown in detail so as not to obscure the understanding of this description.
[0167] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.
Claims
1. A bonded article, characterized in that: The adhesive comprises a first component and a second component; The first component comprises by weight: Epoxy resin, 30-50 parts; Sulfide, 0.1-0.5 parts; Accelerator, 0.1-1 part; Catalyst, 0-0.1 part; Toughener, 3-5 parts; Flame retardant, 3-5 parts; The first solvent, 5-10 parts; The second component comprises by weight: Isocyanate, 30-40 parts; Polyol, 1-10 parts; Second solvent, 5-10 parts.
2. The adhesive according to claim 1, characterized in that The ratio of the first component to the second component ranges from 100:10 to 100:
15.
3. The adhesive according to claim 2, characterized in that The sulfide comprises mercaptan; The accelerator includes at least one of a tertiary amine accelerator and a pyridine accelerator; The catalyst includes a metal catalyst; The toughening agent includes a rubber toughening agent; The flame retardant includes an organic phosphorus flame retardant; The first solvent includes a ketone solvent.
4. The adhesive according to claim 2, characterized in that: The polyols include alcohols containing multiple hydroxyl groups; The second solvent includes a ketone solvent.
5. The bonded article according to any one of claims 1 to 4, characterized in that The peel strength of the adhesive is in the range of 18-32 KN / m; and / or, The bonding temperature range of the adhesive is 1-25°C; and / or, The bonding time of the adhesive is in the range of 10-30 minutes.
6. A bonding layer, characterized in that: The invention comprises the adhesive as claimed in any one of claims 1 to 5.
7. A non-pneumatic tire, characterized in that: The invention comprises a wheel spoke, a tread and the bonding layer as claimed in claim 6, wherein the bonding layer is used for bonding the wheel spoke to the tread.
8. A method for preparing a bonded article according to any one of claims 1 to 5, characterized in that: The steps include: obtaining the first component; obtaining the second component; The first component and the second component are mixed in a ratio of 100:10-100:15 to obtain the adhesive.
9. The adhesive according to claim 8, characterized in that The obtaining of the first component comprises: Dehydrating the epoxy resin at 110-130° C. for 110-130 min to obtain a dehydrated epoxy resin; After cooling the dehydrated epoxy resin to 50-70° C., the sulfide, the toughening agent, the flame retardant and the first solvent are added, and after uniform mixing, the accelerator and the catalyst are added. After reacting for a period of time, the first component is obtained.
10. The adhesive according to claim 8, characterized in that The obtaining of the second component comprises: Dehydrating the polyol at 110-130° C. for 11-13 min to obtain a dehydrated polyol; The dehydrated polyol is cooled to 30-50°C, and the second solvent is added to disperse the dehydrated polyol evenly. The isocyanate is then added to the dehydrated polyol in multiple times, and the reaction is continued for a period of time and the temperature is raised to 75-80°C. After further reaction for a period of time, the temperature is cooled to 25-30°C to obtain the second component.
Citation Information
Patent Citations
Epoxy resin adhesive and preparation method thereof
CN104312508A
Adhesive, its manufacturing method and plastic film-laminated sheet iron
JP2004269679A
Heat-curable epoxy resin composition containing one blocked and one epoxide-terminated polyurethane prepolymer
US20090288766A1
Urethane modified epoxy adhesive composition
WO2001040396A2
Blocked polyurethane impact modifiers for improving the impact strength of low-temperature curing single-component epoxy adhesives
WO2018029311A1