Bio-based polyurethane adhesive and preparation process thereof

By reacting bio-based polyols and activated lignin with isocyanate, bio-based polyurethane adhesives with high bonding and environmental protection are prepared, which solves the problems of pollution and low resource utilization of traditional polyurethane adhesives and achieves environmental protection and efficient bonding effect.

CN119019974APending Publication Date: 2024-11-26GUANGDONG SANQI CHEM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411083499.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional polyurethane adhesives produce a large amount of waste liquid and pollution during the preparation process, and the recycling rate of waste is low, resulting in environmental pollution and waste of resources.

Method used

Use bio-based polyols and activated lignin to replace traditional polyester polyols and polyether polyols. Activated lignin is extracted through lithium hydroxide and ethylene glycol phenyl ether to improve its reaction activity and react with isocyanate to prepare good bonding. Bio-based polyurethane adhesive for performance and environmental protection.

Benefits of technology

It significantly reduces the generation of waste liquid, improves the environmental protection of production, and improves the bonding and degradation properties of bio-based polyurethane adhesives, forms a tight-structured adhesive layer, and reduces environmental pollution and resource waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004984486310000051
    Figure BDA0004984486310000051
  • Figure BDA0004984486310000071
    Figure BDA0004984486310000071
  • Figure BDA0004984486310000081
    Figure BDA0004984486310000081
Patent Text Reader

Abstract

The invention relates to the technical field of polyurethane adhesives, in particular to a bio-based polyurethane adhesive and a preparation process thereof. The invention relates to the technical field of polyurethane adhesives, in particular to a bio-based polyurethane adhesive and a preparation process thereof. The bio-based polyurethane adhesive is prepared from the following raw materials in parts by weight: 60 to 70 parts of isocyanate, 110 to 140 parts of bio-based polyol, 60 to 70 parts of activated lignin, 1 to 3 parts of a catalyst, 1 to 2 parts of a flatting agent, 1 to 2 parts of a stabilizer and 1 to 2 parts of an antioxidant. The bio-based polyurethane adhesive prepared by using the preparation method has good adhesive property, the generation of waste liquid is reduced in the preparation process, and the environmental protection property in the production process is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polyurethane adhesives, and more specifically, to a bio-based polyurethane adhesive and a preparation process thereof. Background Art

[0002] Polyurethane adhesives refer to adhesives containing carbamate groups (-NHCOO-) or isocyanate groups (-NCO) in the molecular chain. They are mainly divided into two categories: single-component polyurethane adhesives and two-component polyurethane adhesives. Single-component polyurethane adhesives are generally composed of terminal NOC-based prepolymers or their encapsulated materials, which react and solidify with active hydrogen-containing components or moisture in the air to produce adhesion; two-component polyurethane adhesives are composed of terminal hydroxyl components (polyurethane-type terminal hydroxyl products formed by polyester or / and polyether polyols and diisocyanates and chain extenders) and terminal NOC components, and have good bonding properties.

[0003] Polyurethane adhesives can be used in textiles, paper, plastics, automobiles, furniture or construction, and my country has a large population, so the demand for polyurethane adhesives in the clothing field is relatively large. Water-based polyurethane adhesives can be widely used to form coatings on the surface of clothing fabrics, protect fabrics and improve more functions such as waterproofing and oil resistance. Especially now that most of the clothes people wear are fast-moving consumer goods, the amount of polyurethane adhesives used is even greater. However, the large-scale use of traditional polyurethane adhesives causes great damage to the environment. First of all, a large amount of waste liquid will be produced in the process of preparing single-component polyurethane adhesives and two-component polyurethane adhesives. The main pollutants in the wastewater are COD (4000mg / L), BOD (1000mg / L), SS (500mg / L) and other substances. It takes a lot of material and financial resources to treat production waste liquid, and the treatment effect is not good. Secondly, the pollution of its product waste to the environment cannot be underestimated. The resource recycling and reuse rate of polyurethane adhesive waste is low, and the process costs of chemical recovery methods such as pyrolysis, ammonialysis, alcoholysis, and alkaline hydrolysis are relatively high; landfill treatment leads to slow natural degradation, resulting in the generation of a large amount of solid waste; incineration produces HCN, CO2, and CO, which can easily cause secondary pollution.

[0004] Therefore, it is extremely important to develop a pollution-free polyurethane adhesive with good bonding properties. Summary of the invention

[0005] In order to improve the problems of high pollution and poor environmental performance of traditional polyurethane adhesives and obtain environmentally friendly adhesives, the present application provides a bio-based polyurethane adhesive and a preparation process thereof.

[0006] In the first aspect, the present application provides a bio-based polyurethane adhesive, which adopts the following technical solution: A bio-based polyurethane adhesive, wherein the bio-based polyurethane adhesive is prepared by including the following raw materials in parts by weight: Bio-based polyol 110-140 parts Activated lignin 60-70 parts Catalyst 1-3 parts 1-2 parts of leveling agent 1-2 parts of stabilizer 1-2 servings of antioxidants.

[0007] By adopting the above technical solution, the bio-based polyurethane adhesive prepared has good bonding performance, and the generation of waste liquid is reduced during the preparation process, thereby improving the environmental protection of the production process. At the same time, the present application uses bio-based polyols and activated lignin to replace the original polyester polyols and polyether polyols, thereby improving the environmental protection of the bio-based polyurethane and further improving the bonding properties of the bio-based polyurethane. Among them, the activated lignin has high reactivity and is easy to react with isocyanate, thereby improving the bonding performance and environmental protection performance of the polyurethane adhesive.

[0008] The general lignin does not react with isocyanate, and when used to prepare polyurethane adhesives, it can only enhance the hardness of polyurethane adhesives, but cannot increase the bonding performance of polyurethane adhesives, and sometimes even reduces the bonding performance of polyurethane adhesives. The activated lignin in this application has more active groups and a small molecular weight, and is easy to react with isocyanate, thereby forming a bio-based polyurethane adhesive with good adhesion and environmental protection.

[0009] Preferably, the catalyst is at least one of triethylamine, triethanolamine, triethylenediamine, propylenediamine, dibutyltin dilaurate or stannous octoate.

[0010] Preferably, the isocyanate is at least one of 4,4',4'-triphenylmethane diisocyanate, 4,4'-triphenylmethane diisocyanate, 2,4-toluene diisocyanate or hexamethylene diisocyanate.

[0011] Preferably, the activated lignin is prepared by the following method: A: Add 20-25 parts of lignin to 40-60 parts of 10-15% lithium hydroxide solution and ethylene glycol phenyl ether, heat to 90-100°C, continue to react for 0.5-1h after the lignin is completely dissolved, add 2-6 parts of saturated sodium chloride solution, separate the layers, and take the organic layer solution; B: Wash the organic layer with 5-10 parts of 5-10% sodium phosphate solution, dry and concentrate to obtain a concentrated solution, and then introduce 3-5 parts of hydrogen chloride gas under the conditions of pressure of 120-130 kPa and temperature of 70-90°C to obtain activated lignin.

[0012] By adopting the above technical solution, the connection mode between the main bodies of the lignin structure is destroyed, and the active groups of the lignin are changed and increased, thereby improving the reactivity of the lignin, which is conducive to reacting with bio-based polyols and isocyanates to form a bio-based polyester adhesive with good bonding properties and environmental protection.

[0013] The ether bonds and carbon-carbon bonds between the main structures of lignin are destroyed by the action of lithium hydroxide solution, the original structure of lignin is changed, and the molecular weight of lignin is reduced. After the main chain structure of lignin is destroyed, the activity of the reactive groups of activated lignin is increased by the reduction action of hydrogen chloride gas. The activated lignin reacts with isocyanate and bio-based polyol to improve the bonding performance of bio-based polyurethane.

[0014] The present application adopts lithium hydroxide solution and ethylene glycol phenyl ether to work together, so that the main chain of lignin is disconnected to expose more functional groups in a low-molecular chain structure, which is conducive to obtaining more activated functional groups later, and more low-molecular-weight lignin can be extracted through the action of ethylene glycol phenyl ether. Traditional lignin extraction includes acid extraction, alkali extraction, organic solvent extraction and high-boiling alcohol solvent extraction. Among them, the dissolution rate obtained by high-boiling alcohol solvent extraction is the highest, at about 65%, and the process is complicated. The lignin extracted by the method of the present application has a simple process and a dissolution rate of up to 83%, and the reaction activity of the activated lignin obtained is good.

[0015] Preferably, the weight ratio of the lithium hydroxide solution to the ethylene glycol phenyl ether is 2:(3-5).

[0016] Preferably, the rate of adding hydrogen chloride gas in step B is 0.01-0.02 Kg / min.

[0017] By adopting the above technical solution, the decomposed lignin can fully contact with the hydrogen chloride gas, thereby improving the activation performance of the lignin, which is conducive to the reaction of the activated lignin with bio-based polyols and isocyanates to form a bio-based polyurethane adhesive with good bonding and degradation properties.

[0018] Preferably, the bio-based polyol has a hydroxyl value of 30-60 mgKOH and a weight average molecular weight of 2000-6000.

[0019] By adopting the above technical scheme, the hydroxyl value and weight-average molecular weight of the bio-based polyol are optimized, the compatibility of component A and component B is further improved, the reaction rate of the bio-based polyol with activated lignin and isocyanate is controlled, and the curing structure of the bio-based polyurethane adhesive is controlled, thereby improving the bonding performance of the bio-based polyurethane adhesive.

[0020] Preferably, the weight ratio of the activated lignin to the isocyanate is 40:(85-90).

[0021] By adopting the above technical solution, the reaction between activated lignin and isocyanate is optimized, and then the structure after the reaction between activated lignin and isocyanate is optimized, and finally the bonding performance of the polyurethane adhesive is improved.

[0022] Preferably, the component A further comprises 10-15 parts by weight of a bio-based polyether polyol, and the functionality of the bio-based polyether polyol is 2-3.

[0023] The above technical solution is used to further improve the bonding performance and degradation performance of the bio-based polyurethane adhesive. Compared with traditional polyether polyols, the above bio-based polyether polyols have the advantages of good degradation performance and low pollution. Traditional polyether polyols are made from petrochemical products, which are highly polluting. Compared with the above bio-based polyether polyols, their carbon chain ends and branching degree are small, and the bonding performance of the bio-based polyurethane adhesive prepared with them is relatively weak.

[0024] Preferably, the bio-based polyether polyol is at least one of soybean oil polyether polyol, palm oil polyether polyol or olive oil polyether polyol.

[0025] Preferably, the leveling agent is a polyacrylate leveling agent or a silicone leveling agent.

[0026] By adopting the above technical solution, the fluidity of component A is improved, so that the compatibility of component A with component B is improved. At the same time, the surface tension of the bio-based polyurethane adhesive can be reduced, the leveling property of the bio-based polyurethane adhesive can be improved, and it is conducive to forming a smooth film layer.

[0027] Preferably, the stabilizer is a polyurethane foam stabilizer.

[0028] By adopting the above technical solution, fewer bubbles can be generated during the mixing and curing of component A and component B. At the same time, the surface tension of the bio-based polyurethane adhesive can be reduced, the stability of the bio-based polyurethane adhesive system can be improved, and the density of the bio-based polyurethane can be made uniform, which is conducive to film formation.

[0029] In a second aspect, the present application provides a method for preparing a bio-based polyurethane adhesive, using the following technical solution: A method for preparing a bio-based polyurethane adhesive comprises the following preparation steps: S1. According to parts by weight, under the protection of nitrogen, add 30-50 parts of bio-based polyol to the reaction, heat to 70-80° C., add isocyanate, control the temperature at 70-80° C., react for 3-4 hours, and obtain bio-based polyurethane; S2. According to the weight percentage, under the protection of nitrogen, the remaining biopolyol is put into the reactor, the temperature is raised to 110-130°C, vacuum dehydration is carried out for 1-3 hours, the temperature is cooled to 70-80°C, activated lignin is added, the temperature is lowered to 60-70°C, stirring is continued for 1-2 hours, the temperature is cooled to 30-40°C, and finally a leveling agent, a stabilizer and a catalyst are added and stirred evenly to obtain a bio-based polyurethane adhesive.

[0030] By adopting the above technical solution, the production efficiency is high, the prepared bio-based polyurethane adhesive has good bonding performance, good degradation performance, low cost in the preparation process, and high environmental protection.

[0031] In summary, this application has the following beneficial effects: 1. The present application prepares a bio-based polyurethane adhesive by using bio-based polyurethane, bio-based polyol, activated lignin, catalyst, leveling agent, stabilizer and antioxidant; uses isocyanate and bio-based polyol to prepare bio-based polyurethane, and then uses the bio-based polyurethane to prepare a bio-based polyurethane adhesive, which has good bonding and degradation properties. Among them, the activated lignin has more active groups, high reactivity and small molecular weight, and is easy to react with isocyanate and bio-based polyol, thereby improving the bonding performance of the bio-based polyurethane adhesive. When using the bio-based adhesive, the activated lignin reacts with isocyanate and bio-based polyol to form a tight adhesive layer. 2. The present application adopts lithium hydroxide solution and ethylene glycol phenyl ether to dissolve and extract lignin, and then obtains a concentrated solution through liquid separation, washing, drying and concentration steps; and then reacts the concentrated solution with hydrogen chloride gas under the conditions of a pressure of 120-130 kPa and a temperature of 70-90 ° C, thereby obtaining activated lignin with high reaction activity. Among them, the lithium hydroxide solution and ethylene glycol phenyl ether act synergistically with each other, so that the main chain of lignin is disconnected to expose more functional groups in a low-molecular chain structure, which is conducive to obtaining more activated functional groups in the subsequent process, and more low-molecular-weight lignin can be extracted through the action of ethylene glycol phenyl ether, and the product rate of activated lignin can reach 83%. DETAILED DESCRIPTION

[0032] Preparation Example 1-3 Preparation Example 1 An activated lignin is prepared by the following method: A: Add 2 kg of lignin to a mixture of 4 kg of 10% lithium hydroxide solution and ethylene glycol phenyl ether, heat to 90 ° C, and continue to react for 0.5 h after the lignin is completely dissolved, add 0.2 kg of saturated sodium chloride solution, separate the layers, and take the organic layer solution; B: Wash the organic layer with 0.5 kg of 5% sodium phosphate solution, dry and concentrate to obtain a concentrated solution, and then introduce 0.3 kg of hydrogen chloride gas under the conditions of pressure of 120 kPa and temperature of 70°C to obtain activated lignin.

[0033] Wherein, the dosage ratio of lithium hydroxide solution to ethylene glycol phenyl ether is 2:3.

[0034] Lignin was purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd. with a CAS number of 9005-53-2.

[0035] Preparation Examples 2 and 3 differ from Preparation Example 1 in that the types, amounts and test parameters of some raw materials are different, and the remaining test steps are consistent with Preparation Example 1. The materials and amounts used in Preparation Examples 1 to 3 are shown in Table 1: Table 1 Materials and amounts used in Preparation Examples 1 to 3 Comparative Preparation Example Comparative Preparation Example 1 An activated lignin, the difference between this comparative preparation example and Preparation Example 1 is that: a sodium hydroxide solution with a mass fraction of 10% is used to replace an equal mass of lithium hydroxide solution, and the remaining raw material types, amounts and experimental step parameters are consistent with Preparation Example 1.

[0036] Comparative Preparation Example 2 An activated lignin, the difference between this comparative preparation example and preparation example 1 is that dimethyl sulfoxide replaces ethylene glycol phenyl ether of equal mass, and the other raw material types, amounts and experimental step parameters are consistent with those of preparation example 1.

[0037] Comparative Preparation Example 3 An activated lignin, the difference between this preparation comparative example and Preparation Example 1 is that: the pressure in step B is 120kpa and the temperature is 40°C, and the other raw material types, amounts and experimental step parameters are consistent with Preparation Example 1.

[0038] The yields of activated lignin in Preparation Examples 1-3 and Comparative Preparation Examples 1-3 are shown in Table 2: Table 2 Yield of activated lignin in Preparation Examples 1-3 and Comparative Preparation Examples 1-3 Preparation Examples and Comparative Preparation Examples Yield (%) Comparative Example 1 83 Comparative Example 2 83 Comparative Example 3 85 Comparative Preparation Example 1 65 Comparative Preparation Example 2 63 Comparative Preparation Example 3 60 Example

[0039] Example 1 A bio-based polyurethane adhesive is prepared by the following method: S1. Under the protection of nitrogen, add 0.6 kg of bio-based polyol (cashew nut shell oil bio-based modified polyol) into the reaction, heat to 70°C, add 0.8 kg of isocyanate (4,4',4'-triphenylmethane diisocyanate), control the temperature at 70°C, react for 3 hours, and obtain bio-based polyurethane; S2. Under nitrogen protection, put 0.5Kg of bio-based polyurethane and 0.8Kg of bio-polyol (cashew nut shell oil bio-based modified polyol) into the reactor, heat to 110°C, vacuum dehydrate for 1h, cool to 70°C, add 0.6Kg of activated lignin, cool to 60°C, continue stirring for 1h, cool to 30°C, and finally add 0.01Kg of leveling agent, 0.01Kg of stabilizer, 0.01Kg of catalyst (triethylamine) and 0.01Kg of antioxidant and stir evenly to obtain a bio-based polyurethane adhesive.

[0040] Cashew nut shell liquid bio-based modified polyol was purchased from Guangzhou Haoyi New Materials Technology Co., Ltd., and the model number was cashew nut shell liquid bio-based modified polyol FX-9014. Bio-based modified castor oil polyol was purchased from Guangzhou Haoyi New Materials Technology Co., Ltd., and the model number was Fantelus Polycin D265 bio-based modified castor oil polyol.

[0041] Polytrimethylene ether glycol was purchased from Guangzhou Haoyi New Materials Technology Co., Ltd. and its model is Korean SKECOPROLH1000 polytrimethylene ether glycol.

[0042] Preparation of activated lignin: Weigh lignin, Ru / Fe3O4 / Mo catalyst and methanol and add them into a high-pressure reactor in turn, protect with nitrogen, pressurize to 3 MPa at room temperature, heat to 200°C, stir evenly with magnetic force, react for 4 hours. After the reaction, cool and depressurize the high-pressure reactor naturally, filter to remove insoluble components, remove all volatiles under vacuum conditions, and obtain an activated lignin oily product.

[0043] The stabilizer was AK-8805 polyurethane foam stabilizer, which was purchased from Shandong Huibang New Material Technology Co., Ltd.

[0044] The leveling agent is a polyacrylate leveling agent, the brand is Dow Corning, and the model is DC-51.

[0045] The antioxidant was antioxidant 264.

[0046] The difference between Examples 2-4 and Example 1 is that the types, amounts and test parameters of some raw materials are different, and the remaining test steps are consistent with those of Example 1. The materials and amounts used in Examples 1-4 are shown in Table 3: Table 3 Materials and dosage used in Examples 1-4 Example 5 A bio-based polyurethane adhesive. The difference between this embodiment and embodiment 1 is that the hydroxyl value of the cashew nut shell oil bio-based modified polyol is 30 mgKOH, the weight average molecular weight is 2000, and the remaining raw material types, amounts and experimental steps are consistent with embodiment 1.

[0047] Example 6 A bio-based polyurethane adhesive. The difference between this embodiment and embodiment 2 is that the hydroxyl value of the cashew nut shell oil bio-based modified polyol is 60 mgKOH, the weight average molecular weight is 6000, and the remaining raw material types, amounts and experimental steps are consistent with embodiment 2.

[0048] Example 7 A bio-based polyurethane adhesive. The difference between this embodiment and embodiment 1 is that the weight ratio of activated lignin to isocyanate is 40:85, that is, the amount of activated lignin is 0.4 kg, and the amount of isocyanate (4,4',4"-triphenylmethane diisocyanate) is 0.85 kg. The remaining raw material types, amounts and experimental steps are consistent with those in embodiment 1.

[0049] Example 8 A bio-based polyurethane adhesive. The difference between this embodiment and embodiment 2 is that the weight ratio of activated lignin to isocyanate is 40:90, that is, the amount of activated lignin is 0.4 kg, and the amount of isocyanate (4,4',4'-triphenylmethane diisocyanate) is 0.9 kg. The remaining raw material types, amounts and experimental steps are consistent with embodiment 2.

[0050] Example 9 A bio-based polyurethane adhesive. The difference between this embodiment and embodiment 1 is that component A also includes 0.1 kg of bio-based polyether polyol, the functionality of the bio-based polyether polyol is 2, and the remaining raw material types, amounts and experimental steps are consistent with embodiment 1.

[0051] The bio-based polyether polyol was soybean oil polyether polyol purchased from Wuhan Shiquanxing New Materials Technology Co., Ltd., model number W1162.

[0052] Example 10 A bio-based polyurethane adhesive. The difference between this embodiment and embodiment 2 is that component A also includes 0.15 kg of bio-based polyether polyol, and the remaining raw material types, amounts and experimental steps are consistent with those in embodiment 2.

[0053] The bio-based polyether polyol was soybean oil polyether polyol purchased from Wuhan Shiquanxing New Materials Technology Co., Ltd., model number W1162.

[0054] Embodiment 11 A bio-based polyurethane adhesive. The difference between this embodiment and embodiment 2 is that the activated lignin comes from comparative preparation example 1, and the other raw material types, amounts and experimental steps are consistent with those of embodiment 2.

[0055] Example 12 A bio-based polyurethane adhesive. The difference between this embodiment and embodiment 2 is that the activated lignin comes from comparative preparation example 2, and the remaining raw material types, amounts and experimental steps are consistent with those of embodiment 2.

[0056] Example 13 A bio-based polyurethane adhesive. The difference between this embodiment and embodiment 2 is that the activated lignin comes from comparative preparation example 3, and the remaining raw material types, amounts and experimental steps are consistent with embodiment 2.

[0057] Comparative Example Comparative Example 1 A bio-based polyurethane adhesive. The difference between this embodiment and embodiment 1 is that polyether polyol is used to replace an equal amount of activated lignin, and the remaining raw material types, amounts and experimental steps are consistent with those in embodiment 1.

[0058] Comparative Example 2 A bio-based polyurethane adhesive. The difference between this embodiment and embodiment 1 is that polyether polyol is used instead of an equal amount of bio-based polyol, and the remaining raw material types, amounts and experimental steps are consistent with those in embodiment 1.

[0059] Comparative Example 3 A bio-based polyurethane adhesive. The difference between this embodiment and embodiment 1 is that polyether polyol is used to replace the same amount of activated lignin and bio-based polyol, and the remaining raw material types, amounts and experimental steps are consistent with those in embodiment 1.

[0060] Performance testing The bio-based polyurethane adhesives prepared in Examples 1-13 and Comparative Examples 1-3 were subjected to bonding performance tests and degradation tests.

[0061] Detection method / test method The bio-based polyurethane adhesives prepared in Examples 1-13 and Comparative Examples 1-3 were coated on the surface of the fabric, cured and dried, with a dry thickness of 0.01 mm, and the bonding performance test was performed. The fabric was purchased from Guangzhou Duxian New Materials Co., Ltd., the main component of which was polyethylene, and the brand was Duxian.

[0062] Adhesion firmness test: refer to GB / T21196.1-2007, using the friction resistance method. Under the same conditions, the more friction resistance times, the better the coating firmness.

[0063] Degradation test, using outdoor soil burial degradation test method: the bio-based polyurethane adhesive prepared in Examples 1-13 and Comparative Examples 1-3 is coated on the surface of release paper, and the thickness after curing and drying is 1mm. The release paper is torn off, and a size of 20mm*20mm is cut, and its weight is weighed as m0. It is buried about 10cm under ordinary gardening soil at a certain interval. After it is allowed to degrade under natural conditions for 90 days, the sample is taken out, washed with deionized water, and then placed in a 50℃ forced air drying oven for 24h for drying. Finally, it is balanced at room temperature for 24h, and its weight is weighed again as m1. The weight loss rate of the foam is calculated (weight loss rate = (m0-m1) / m0×100%). The test data are shown in Table 4: Table 4 Performance test data Examples or Comparative Examples Wear test (times) Weight loss rate (%) Example 1 2000 12.3 Example 2 3000 16.7 Example 3 3000 16.8 Example 4 3000 16.8 Example 5 2200 14.3 Example 6 3200 19.2 Example 7 2300 12.9 Example 8 3300 17.3 Example 9 2500 12.4 Example 10 3500 16.7 Embodiment 11 2100 14.3 Example 12 2100 12.3 Example 13 1800 11.1 Comparative Example 1 1600 5.6 Comparative Example 2 1900 3.1 Comparative Example 3 1400 0.5 From Examples 1-13 and Comparative Examples 1-3 in combination with Table 4, it can be seen that by preparing component A from bio-based polyols, activated lignin, catalysts, leveling agents, stabilizers and antioxidants; preparing component B from bio-based polyols and isocyanates; and then preparing a bio-based polyurethane adhesive from component A and component B, the friction resistance is no less than 2000 times, and the weight loss rate is greater than 12.3%, indicating that the bio-based polyurethane adhesive prepared by the present application has good bonding properties and degradation properties.

[0064] Comparison between Example 1 and Comparative Examples 1-3 shows that the use of bio-based polyols and activated lignin can improve the degradation performance of the bio-based adhesive, while also maintaining the good bonding performance of the bio-based polyurethane adhesive.

[0065] Comparison between Example 1 and Examples 2-3 and 11-13 shows that by preparing activated lignin using the preparation method in the present application, the bonding performance and degradation performance of the bio-based polyurethane adhesive can be further improved. In combination with Table 2, it can be seen that the yield of activated lignin obtained by the preparation method of the present application is high.

[0066] Comparison between Example 1 and Examples 5 and 7 indicates that optimizing the ratio of the amount of bio-based polyol and activated lignin to isocyanate in the present application can further improve the bonding performance and degradation performance of the bio-based polyurethane adhesive.

[0067] Comparison between Example 1 and Example 9 shows that by adding a bio-based polyether polyol with a functionality of 2 to component A, the bonding performance and degradation performance of the bio-based polyurethane adhesive can be further improved.

[0068] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A bio-based polyurethane adhesive, characterized in that: The bio-based polyurethane adhesive is prepared by including the following raw materials in parts by weight: Bio-based polyol 110-140 parts Activated lignin 60-70 parts Catalyst 1-3 parts 1-2 parts of leveling agent 1-2 parts of stabilizer 1-2 servings of antioxidants.

2. A bio-based polyurethane adhesive according to claim 1, characterized in that: The activated lignin is prepared by the following method: Add 20-25 parts of lignin to 10-15% by mass lithium hydroxide solution and ethylene glycol phenyl ether, heat to 90-100°C, continue to react for 0.5-1h after the lignin is completely dissolved, add saturated sodium chloride solution, separate the layers, and take the organic layer solution; The organic layer is washed with a sodium phosphate solution with a mass fraction of 5-10%, dried, and concentrated to obtain a concentrated solution. Under the conditions of a pressure of 120-130 kPa and a temperature of 70-90° C., 3-5 parts of hydrogen chloride gas are introduced to obtain activated lignin.

3. A bio-based polyurethane adhesive according to claim 2, characterized in that: The weight ratio of the lithium hydroxide solution to the ethylene glycol phenyl ether is 2:(3-5).

4. The bio-based polyurethane adhesive according to claim 1, characterized in that: The bio-based polyol has a hydroxyl value of 30-60 mgKOH and a weight average molecular weight of 2000-6000.

5. The bio-based polyurethane adhesive according to claim 1, characterized in that: The weight ratio of the activated lignin to the isocyanate is 40:(85-90).

6. The bio-based polyurethane adhesive according to claim 1, characterized in that: The component A further comprises 10-15 parts by weight of a bio-based polyether polyol, wherein the functionality of the bio-based polyether polyol is 2-3.

7. The bio-based polyurethane adhesive according to claim 1, characterized in that: The leveling agent is a polyacrylate leveling agent or an organosilicon leveling agent.

8. The bio-based polyurethane adhesive according to claim 1, characterized in that: The stabilizer is a polyurethane foam stabilizer.

9. A method for preparing the bio-based polyurethane adhesive according to any one of claims 1 to 8, characterized in that: The method comprises the following preparation steps: S1. According to parts by weight, under the protection of nitrogen, add 30-50 parts of bio-based polyol to the reaction, heat to 70-80° C., add isocyanate, control the temperature at 70-80° C., react for 3-4 hours, and obtain bio-based polyurethane; S2. According to the weight percentage, under the protection of nitrogen, the remaining biopolyol is put into the reactor, the temperature is raised to 110-130°C, vacuum dehydration is carried out for 1-3 hours, the temperature is cooled to 70-80°C, activated lignin is added, the temperature is lowered to 60-70°C, stirring is continued for 1-2 hours, the temperature is cooled to 30-40°C, and finally a leveling agent, a stabilizer and a catalyst are added and stirred evenly to obtain a bio-based polyurethane adhesive.