Crack plugging fluid for casing-in-casing solid casing well and casing-in-casing solid casing well cementation method
By using water, polypropylene fiber, walnut shell and pH-responsive hydrophobic assembled sealant in shale gas wells, the problem of crack sealing after primary fracturing in shale gas wells is solved, and rapid and efficient The leakage plugging effect shortens the construction cycle and reduces costs, ensuring the safety and efficiency of cementing.
Patent Information
- Application Number
- CN202410995873.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-24
AI Technical Summary
In shale gas wells, the original cracks after the initial fracturing are difficult to effectively seal, resulting in loss of cement slurry during the cementing process, affecting the safety of cementing. Moreover, traditional leak-blocking materials are difficult to form a tight sealing and plugging layer, and the leak-blocking effect is not good. And the wells that do not require unblocking have a long construction cycle and high cost.
A leak-blocking liquid including water, polypropylene fiber, walnut shell and pH-responsive hydrophobic associative sealant is used to bridge the cracks through the complexation of walnut shell and fibers, and the pH-responsive hydrophobic associative sealant is used to seal it. The thixotropic properties of the plugging agent are fast pumped under acidic conditions, and the viscosity increases the sealing effect under alkaline conditions. The calcium ion cross-linking of the cementing cement slurry forms a gel to achieve rapid and efficient sealing.
It realizes that cementing construction is carried out directly without long wait, shortening the construction cycle, reducing costs, improving leakage plugging effect and cementing quality, and ensuring the safety and efficiency of the solid-sleeved well in the sleeve.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil and gas wells, and in particular to a casing-in-casing well crack plugging liquid and a casing-in-casing cementing method. Background Art
[0002] Shale gas reservoirs have the characteristics of low porosity, low permeability, and no natural production capacity. Its efficient development requires the use of large-scale hydraulic fracturing to form artificial fractures to provide seepage channels for production, but there are problems such as rapid production decline and short stable production period after the initial transformation. It is necessary to run a small casing into the original wellbore, cement the small casing, and then perform repeated fracturing to increase the production capacity of shale gas wells again.
[0003] The technology of inserting small casing into old shale gas wells for cementing is called casing-in-casing technology. Since there are original cracks from the initial fracturing in old shale gas wells, the original cracks need to be sealed before the casing-in-casing cementing operation to prevent cement slurry from leaking into the cracks during the cementing process and affecting the safety of cementing. The original cracks formed by the initial fracturing are numerous, deep, and have low pressure inside the cracks, making the plugging operation difficult. It is difficult to form a tight plugging layer in the cracks using traditional bridging plugging materials, and the plugging effect is difficult to meet the requirements. For this reason, it is of great significance to research and develop a plugging fluid system with good plugging ability.
[0004] For wells that need to remove the plugging liquid in the cracks after cementing, the use of water-absorbing resin as the main agent of the plugging liquid has significant advantages. When unblocking is required, peroxidants (such as ammonium persulfate, etc.) can be used to decompose the water-absorbing resin to remove the blockage. Although the water-absorbing resin has significant advantages in unblocking, in order to improve the plugging ability of the water-absorbing resin, it is necessary to continue to inject sodium hydroxide alkali solution after injecting the plugging liquid into the cracks, and wait for 24 hours or more before cementing construction, resulting in an extension of the construction time, which in turn leads to an increase in costs. For wells that do not need to be unblocked after plugging, it is of great significance to develop a plugging liquid and plugging method with good plugging effect and short construction period. Summary of the invention
[0005] The purpose of the present invention is to solve the above technical problems and provide a casing-in-casing well crack plugging liquid with simple ingredients, easy availability, low cost and good plugging effect.
[0006] The invention also provides a casing-in-casing cementing method with simple method, easy operation, good plugging effect and short construction period.
[0007] The casing-in-casing well crack plugging liquid of the present invention comprises the following components in parts by weight: water: 100 parts, polypropylene fiber: 0.4-1 parts, walnut shell: 4-9 parts, pH-responsive hydrophobic associating plugging agent: 2-5 parts, and defoaming agent: 1-4 parts.
[0008] The pH-responsive hydrophobic associating plugging agent is prepared by uniformly mixing 100 parts of water, 16 parts of acrylic acid, 4 parts of methacrylic acid, 4.75 parts of vinyl pyridine, 0.25 parts of dodecyl methacrylate, 1 part of urea, and 0.3 parts of ammonium persulfate, curing at 60° C. for 4 hours, and then drying and crushing.
[0009] The defoamer is a polyether defoamer or a silicone defoamer.
[0010] The length of the polypropylene fiber is 0.8-1.2 mm.
[0011] The particle size of the walnut shell is 2-3 mm.
[0012] The casing-in-casing cementing method of the present invention comprises the following steps: pumping the crack plugging liquid to the bottom of the well; continuously squeezing the plugging liquid into the formation cracks after the well is shut down until the pump pressure reaches 5-6 MPa; and then pumping cement slurry into the annulus of the downhole casing to make the cement slurry contact and react with the plugging liquid in the cracks until the cement slurry solidifies.
[0013] The crack plugging liquid is pumped to the bottom of the well, and the well is shut down when it is pumped to 200-500m above the leaking layer.
[0014] Pump cementing slurry into the annulus of the casing downhole until the cementing slurry returns to the preset position.
[0015] The cementing slurry is silicate cement slurry.
[0016] In view of the problems existing in the background technology, a casing well crack plugging liquid that can be used for rapid plugging construction is designed for wells that do not need to be unblocked after plugging, wherein (1) the walnut shell and fiber in the plugging liquid work together to bridge and plug the perforation holes and formation cracks. The reason for using the two in combination is that the walnut shell has a high strength and can play a good supporting and bridging role in the cracks, and the fiber can fill the gaps between the walnut shell particles. Compared with using them alone, the composite can better achieve efficient plugging of cracks. (2) A pH-responsive hydrophobic associating plugging agent is introduced into the solid technology, so that the plugging liquid containing the plugging agent has thixotropy. It contains a large number of carboxylic acid groups and has a low viscosity under acidic conditions. Therefore, it has good fluidity when pumped, can be quickly transported to the well and smoothly enter the cracks. After plugging the cracks and perforations, the cementing slurry subsequently fed in is alkaline. After contacting with the cementing slurry, the viscosity of the pH-responsive hydrophobic associating plugging agent will increase significantly under neutral and alkaline conditions, thereby effectively enhancing the plugging effect and ensuring the quality of cementing. By using the above principle, after injecting the plugging fluid, there is no need to wait for a long time, and cementing slurry can be directly injected for cementing construction, thereby greatly shortening the construction period; (3) The carboxylic acid groups in the pH-responsive hydrophobic associating plugging agent will also undergo cross-linking under the action of calcium ions, so that the pH-responsive hydrophobic associating plugging agent cross-links to form a gel, which is very beneficial to the improvement of the plugging ability of the plugging fluid. Among them, the amount of pH-responsive hydrophobic associating plugging agent should be controlled at 2-5 parts. Too much will cause the loss of the plugging fluid to be difficult to meet the construction requirements, and too little will result in poor thixotropy.
[0017] The present invention adds a pH-responsive hydrophobic associating plugging agent to the plugging liquid, and skillfully combines it with cementing cement slurry, which can ensure the flowability of the plugging liquid during pumping and greatly improve the anti-leakage ability during plugging, thereby ensuring the cementing quality of the casing-in-casing well. After plugging, cementing construction can be directly carried out. The cementing method of the present invention has a short construction period, is extremely simple to operate, is low in cost, and has a good plugging effect. DETAILED DESCRIPTION
[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the embodiments or the prior art will be briefly introduced below. Obviously, the following descriptions are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these embodiments without creative work. The parts in the following embodiments are parts by weight.
[0019] Example 1
[0020] Preparation of plugging agent: prepare plugging liquid according to 100 parts of water, 0.4 parts of polypropylene fiber, 4 parts of walnut shell, 2 parts of pH responsive hydrophobic associating plugging agent and 1 part of defoaming agent;
[0021] The pH-responsive hydrophobic associating plugging agent is prepared by uniformly mixing 100 parts of water, 16 parts of acrylic acid, 4 parts of methacrylic acid, 4.75 parts of vinyl pyridine, 0.25 parts of dodecyl methacrylate, 1 part of urea, and 0.3 parts of ammonium persulfate, curing at 60°C for 4 hours, and then drying and crushing.
[0022] Experiment: The viscosity of the prepared plugging liquid is 10Pa·S in the initial state. After adding 3 parts of cement, the viscosity of the plugging liquid is 195Pa·S.
[0023] In a shale gas well with a depth of 3,800 meters, before the casing-in-casing cementing operation, the plugging liquid is first pumped to the bottom of the well using a continuous oil pipe, and the well is shut down after being pumped to 200 meters above the leaking layer. After shutting in the well, the plugging liquid is continuously squeezed into the formation cracks until the pump pressure reaches 5 MPa; the cementing slurry is pumped into the annulus of the casing downhole until the cementing slurry returns to the preset position.
[0024] Later logging calculations showed that the cement slurry loss was 0.1m 3 , the cement slurry loss is small and the cementing construction is smooth.
[0025] Example 2
[0026] Preparation of plugging agent: 100 parts of water, 0.7 parts of polypropylene fiber, 6 parts of walnut shells, 4 parts of pH-responsive hydrophobic associating plugging agent, and 2 parts of defoaming agent; the preparation of the pH-responsive hydrophobic associating plugging agent is the same as that in Example 1.
[0027] Experiment: The viscosity of the prepared plugging liquid is 15Pa·S in the initial state. After adding 3 parts of cement into the plugging liquid, the viscosity of the plugging liquid is 290Pa·S.
[0028] In a shale gas well with a depth of 3,900 meters, before the casing-in-casing cementing operation, the plugging liquid was pumped to the bottom of the well using a continuous tubing, and the well was shut down at 500 meters above the leaking layer. After shutting in the well, the plugging liquid was continuously squeezed into the formation cracks until the pump pressure reached 6 MPa; the cementing slurry was pumped into the annulus of the casing downhole until the cementing slurry returned to the preset position.
[0029] Later logging calculations showed that the cement slurry loss was 0.1m 3 , the cement slurry loss is small and the cementing construction is smooth.
[0030] Example 3
[0031] Preparation of plugging agent: prepare plugging liquid according to 100 parts of water, 1 part of polypropylene fiber, 9 parts of walnut shells, 5 parts of pH-responsive hydrophobic associating plugging agent and 3 parts of defoaming agent; the preparation of the pH-responsive hydrophobic associating plugging agent is the same as that in Example 1.
[0032] The viscosity of the prepared plugging liquid is 18 Pa·S in the initial state. After 3 parts of cement are added to the plugging liquid, the viscosity of the plugging liquid is 335 Pa·S.
[0033] In a shale gas well with a depth of 4,200 meters, before the casing-in-casing cementing operation, the plugging liquid was first pumped to the bottom of the well using a continuous tubing, and the well was shut down after being pumped to 400 meters above the leaking layer; after shutting in the well, the plugging liquid was continued to be squeezed into the formation cracks until the pump pressure reached 6 MPa; the cementing slurry was pumped into the annulus of the casing downhole until the cementing slurry returned to the preset position.
[0034] Later logging calculations showed that the cement slurry loss was 0.06m 3 , the cement slurry loss is small and the cementing construction is smooth.
[0035] Comparative Example 1
[0036] Preparation of plugging agent: prepare plugging liquid according to 100 parts of water, 0.4 parts of polypropylene fiber, 4 parts of walnut shells, 3 parts of polyacrylamide and 1 part of defoaming agent.
[0037] Experiment: The viscosity of the prepared plugging liquid is 10Pa·S in the initial state. After adding 3 parts of cement into the plugging liquid, the viscosity of the plugging liquid is 12Pa·S.
[0038] A shale gas well with a depth of 3,800 meters, and the specific method is the same as that in Example 1.
[0039] Later logging calculations showed that the cement slurry loss was 3m 3 The leakage is large, which is very unfavorable for cementing construction.
[0040] Comparative Example 2
[0041] Preparation of plugging agent: prepare plugging liquid according to 100 parts of water, 0.8 parts of polypropylene fiber, 6 parts of walnut shells, 4 parts of polyacrylamide and 1 part of defoaming agent.
[0042] Experiment: The viscosity of the prepared plugging liquid is 13Pa·S in the initial state. After adding 3 parts of cement into the plugging liquid, the viscosity of the plugging liquid is 15Pa·S.
[0043] A shale gas well with a depth of 3900 meters, the specific method is the same as that of Example 2.
[0044] Later logging calculations showed that the cement slurry loss was 2m 3 The leakage is large, which is very unfavorable for cementing construction.
[0045] Comparative Example 3
[0046] Preparation of plugging agent: prepare plugging liquid according to 100 parts of water, 0.8 parts of polypropylene fiber, 6 parts of walnut shells, 7 parts of pH responsive hydrophobic associating plugging agent and 1 part of defoaming agent.
[0047] Since the amount of pH-responsive hydrophobic associating plugging agent added was too large, the plugging liquid had too high viscosity, which made it difficult to prepare the plugging liquid and made it impossible to pump it.
Claims
1. A casing-in-casing well crack plugging fluid, characterized in that: The invention comprises the following components in parts by weight: 100 parts of water, 0.4-1 parts of polypropylene fiber, 4-9 parts of walnut shell, 2-5 parts of pH-responsive hydrophobic association plugging agent and 1-4 parts of defoaming agent.
2. The casing-in-casing well crack plugging liquid according to claim 1, characterized in that: The pH-responsive hydrophobic associating plugging agent is prepared by uniformly mixing 100 parts of water, 16 parts of acrylic acid, 4 parts of methacrylic acid, 4.75 parts of vinyl pyridine, 0.25 parts of dodecyl methacrylate, 1 part of urea, and 0.3 parts of ammonium persulfate, curing at 60° C. for 4 hours, and then drying and crushing.
3. The casing-in-casing well crack plugging liquid according to claim 1 or 2, characterized in that: The defoamer is a polyether defoamer or a silicone defoamer.
4. The casing-in-casing well crack plugging liquid according to claim 1 or 2, characterized in that: The length of the polypropylene fiber is 0.8-1.2 mm.
5. The casing-in-casing well crack plugging liquid according to claim 1 or 2, characterized in that: The particle size of the walnut shell is 2-3 mm.
6. A casing-in-casing cementing method, characterized in that: The crack plugging liquid according to any one of claims 1 to 5 is pumped to the bottom of the well; after the well is shut down, the plugging liquid is continuously squeezed into the formation cracks until the pump pressure reaches 5-6 MPa; then cementing slurry is pumped into the annulus of the downhole casing to make the cementing slurry contact and react with the plugging liquid in the cracks until the cement slurry solidifies.
7. The casing-in-casing cementing method according to claim 6, characterized in that: The fracture plugging liquid is pumped to the bottom of the well, and the well is shut down when the well is pumped to 200-500m above the leaking layer.
8. The casing-in-casing cementing method according to claim 6, characterized in that: Pump cementing slurry into the downhole casing annulus until the cementing mud returns to the preset position.
9. The casing-in-casing cementing method according to any one of claims 6 to 8, characterized in that: The cementing slurry is silicate cement slurry.
Citation Information
Patent Citations
Leak-stopping agent for oil-base drilling fluid
CN105441044A
Hydrophobic associated polymer and preparation method thereof
CN105646777A
Plugging slurry for enhancing pressure-bearing capacity of leakage formation and preparation method thereof
CN106566499A
Water-based drilling fluid plugging agent
CN106609128A
Rigid plugging agent for drilling fluid and preparation method thereof
CN110564383A