Etching composition for silicon nitride layer, method for etching silicon nitride layer using same, and silicon nitride layer

By using an etching composition containing phosphoric acid and specific silane-based compounds in the semiconductor manufacturing process, the problems of selective etching of silicon nitride layer and bubble generation are solved, and efficient silicon nitride layer etching and selective etching of silicon oxide layer are achieved. , improves process efficiency.

CN119020038APending Publication Date: 2024-11-26SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410650876.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-05-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Prior Art In semiconductor manufacturing processes, it is difficult to selectively etch the silicon nitride layer without etching the silicon oxide layer, and bubbles are easily generated due to physical friction when using silane compound etchant, which affects the process efficiency.

Method used

An etching composition containing phosphoric acid, a specific silane-based compound and water is used to adjust the composition and water content of the compound, bubbles generated by physical friction are reduced, and the etching selectivity of the silicon nitride layer to the silicon oxide layer is improved.

Benefits of technology

It effectively reduces bubble generation, shortens the heating time of the etching composition, improves the etching selectivity of the silicon nitride layer on the silicon oxide layer, prevents abnormal growth of the silicon oxide layer, and improves the etching process efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020038A_ABST
    Figure CN119020038A_ABST
Patent Text Reader

Abstract

An etching composition for a silicon nitride layer includes: phosphoric acid; a compound represented by Chemical Formula 1; a compound represented by Chemical Formula 2; and water. In addition, a method for etching a silicon nitride layer includes contacting a surface of the silicon nitride layer with an etching composition for the silicon nitride layer and a silicon nitride layer includes an etched surface etched by the etching composition. Chemical formula 1 (R1) a (R2) b (CH3) Si-(OR3) (3-a-b) chemical formula 2 (R5) c (R6) d (R7) Si-(OR8) (3-c-d).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2023-0067887 filed in the Korean Intellectual Property Office on May 25, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0003] One or more embodiments of the present disclosure relate to an etching composition for a silicon nitride layer, a method for etching a silicon nitride layer using the etching composition, and the silicon nitride layer. Background Art

[0004] Various semiconductor manufacturing processes require a selective etching process for a silicon nitride layer. Recently, for a vertical-NAND (V-NAND) manufacturing process, the development of a process for selectively removing only the silicon nitride layer from a structure in which silicon nitride layers and silicon oxide layers are alternately stacked, and the development of an etching composition solution for implementing the process are being actively explored. Summary of the invention

[0005] One or more aspects of the embodiments of the present disclosure are directed to an etching composition for a silicon nitride layer that can reduce bubbles generated by physical friction.

[0006] One or more aspects of the embodiments of the present disclosure are directed to an etching method using an etching composition for a silicon nitride layer.

[0007] Additional aspects will be set forth in part in the description which follows and, in part, will be obvious from the description, or may be learned by practice of the presented embodiments of the disclosure.

[0008] According to one or more embodiments of the present disclosure, an etching composition for a silicon nitride layer comprises: phosphoric acid; a compound represented by Chemical Formula 1; a compound represented by Chemical Formula 2; and water, wherein the etching composition comprises about 11 wt % to about 16 wt % of water based on the total weight of the etching composition, and in a proton nuclear magnetic resonance (H-NMR) spectrum of the etching composition, the Si-OR a (where R a The ratio of the area of ​​the peak derived from Si-CH3 to the area of ​​the peak derived from Si-CH3 is about 2 to about 16:

[0009] Chemical formula 1

[0010] (R 1 ) a (R2 ) b (CH3)Si-(OR 3 ) (3-a-b) ,

[0011] In Chemical Formula 1,

[0012] R 1 and R 2 may be independently hydrogen, deuterium or a substituted or unsubstituted C1 to C10 alkyl group, R 3 may be each independently a substituted or unsubstituted C1 to C10 alkyl group,

[0013] a and b may each independently be an integer from 0 to 2, and 0≤a+b≤2;

[0014] Chemical formula 2

[0015] (R 5 ) c (R 6 ) d (R 7 )Si-(OR 8 ) (3-c-d) ,

[0016] In chemical formula 2,

[0017] R 5 and R 6 can be independently hydrogen, deuterium, C1 to C10 alkyl, one or more hydrogen atoms are replaced by -NR c R d or a C1 to C10 alkyl group, or a C2 to C10 alkyl group wherein at least one -CH2- in the C2 to C10 alkyl group is replaced by -NR e – the group obtained by substitution,

[0018] R 7 One or more hydrogens may be -NR c R d or a C1 to C10 alkyl group, or a C2 to C10 alkyl group wherein at least one -CH2- in the C2 to C10 alkyl group is replaced by -NR e – the group obtained by substitution,

[0019] R c To R e may each independently be hydrogen, substituted or unsubstituted C1 to C5 alkyl, substituted or unsubstituted C3 to C10 cycloalkyl, substituted or unsubstituted C6 to C10 aryl, or a combination thereof (e.g., any suitable combination),

[0020] R 8 may be a substituted or unsubstituted C1 to C10 alkyl group,

[0021] c and d may each independently be one of integers from 0 to 2, and 0≤c+d≤2.

[0022] In one or more embodiments, in Chemical Formula 1, R 1 To R 3 Each independently may be a substituted or unsubstituted C1 to C5 alkyl group.

[0023] In one or more embodiments, in Chemical Formula 1, R 3 It can be methyl, ethyl or propyl.

[0024] In one or more embodiments, a+b in Chemical Formula 1 may be 0.

[0025] In one or more embodiments, in Chemical Formula 2, R 5 To R 7 Each independently may be one or more hydrogen atoms -NR c R d or a C1 to C10 alkyl group, or a C2 to C10 alkyl group wherein at least one -CH2- in the C2 to C10 alkyl group is replaced by -NR e - The group obtained by substitution.

[0026] In one or more embodiments, R c To R e Each may independently be hydrogen, a substituted or unsubstituted C1 to C5 alkyl group, or a combination thereof (eg, any suitable combination).

[0027] In one or more embodiments, c+d in Chemical Formula 2 is 0.

[0028] In one or more embodiments, the water content (eg, amount) is about 12 wt % to about 15 wt % based on the total weight of the etching composition.

[0029] In one or more embodiments, the Si-OR a (where R a The ratio of the area of ​​the peak derived from Si-CH 3 (which is a substituted or unsubstituted alkyl group) to the area of ​​the peak derived from Si-CH 3 is about 2 to about 10.

[0030] In one or more embodiments, the content (eg, amount) of the compound represented by Chemical Formula 1 is about 0.3 wt % to about 10 wt % based on the total weight of the etching composition.

[0031] In one or more embodiments, the content (eg, amount) of the compound represented by Chemical Formula 2 is about 0.5 wt % to about 30 wt % based on the total weight of the etching composition.

[0032] According to one or more embodiments, a method for etching a silicon nitride layer includes contacting a surface of the silicon nitride layer with an etching composition for the silicon nitride layer.

[0033] According to one or more embodiments, a silicon nitride layer includes: an etched surface etched by an etching composition.

[0034] The etching composition for a silicon nitride layer according to one or more embodiments may reduce bubbles generated by physical friction and shorten the time (eg, duration) taken to heat the etching composition to an etching temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Various features will become apparent to those skilled in the art by describing in detail exemplary embodiments with reference to the accompanying drawings, in which:

[0036] Figure 1 is the etching composition for silicon nitride layer according to Example 1 1 H-NMR spectrum. DETAILED DESCRIPTION

[0037] The exemplary embodiments of the present disclosure will be described in more detail below, and those skilled in the art can easily implement the exemplary embodiments with reference to the described embodiments. However, the present disclosure can be implemented in many different forms and is not to be construed as being limited to the exemplary embodiments set forth herein.

[0038] If no definition is otherwise provided (e.g., when no definition is otherwise provided), "substituted" as used herein may refer to a compound where a hydrogen atom is replaced by a substituent selected from the following: deuterium, halogen (fluorine (F), bromine (Br), chlorine (Cl), or iodine (I)), hydroxyl, nitro, cyano, amino, azido, amidino, hydrazine, hydrazone, carbonyl, carbamoyl, thiol, ester, carboxyl or a salt thereof, sulfonic acid, or a salt thereof, a phosphoric acid or a salt thereof, a C1 to C30 alkyl group, a C2 to C30 alkenyl group, a C2 to C30 alkynyl group, a C6 to C30 aryl group, a C7 to C30 arylalkyl group, a C1 to C30 alkoxy group, a C1 to C20 heteroalkyl group, a C3 to C20 heteroarylalkyl group, a C3 to C30 cycloalkyl group, a C3 to C15 cycloalkenyl group, a C6 to C15 cycloalkynyl group, a C2 to C30 heterocyclyl group and / or combinations thereof (e.g., any suitable combination).

[0039] In one or more embodiments, two adjacent substituents selected from the following may be fused (e.g., bonded to each other) to form (or provide) a ring: substituted halogen (F, Br, Cl, or I), hydroxyl, nitro, cyano, amino, azido, amidino, hydrazine, hydrazone, carbonyl, carbamoyl, sulfhydryl, ester, carboxyl or a salt thereof, sulfonic acid or a salt thereof, phosphoric acid or a salt thereof, C1 to C30 alkyl, C2 to C30 alkenyl, C2 to C30 alkynyl, C6 to C30 aryl, C7 to C30 arylalkyl, C1 to C30 alkoxy, C1 to C20 heteroalkyl, C3 to C20 heteroarylalkyl, C3 to C30 cycloalkyl, C3 to C15 cycloalkenyl, C6 to C15 cycloalkynyl, and C2 to C30 heterocyclyl.

[0040] As used herein, "aryl" may refer to a group including at least one hydrocarbon aromatic moiety, and may include hydrocarbon aromatic moieties linked by a single bond and hydrocarbon aromatic moieties fused directly or indirectly to provide a non-aromatic fused ring. The aryl group may include a monocyclic functional group, a polycyclic functional group, or a fused polycyclic (i.e., rings that share adjacent pairs of carbon atoms) functional group.

[0041] For example, the substituted or unsubstituted aryl group may be a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted phenanthrenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted pyrenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted terphenyl group, a substituted or unsubstituted quaterphenyl group, a substituted or unsubstituted The present invention may be a substituted or unsubstituted triphenylene group, a substituted or unsubstituted perylene group, a combination thereof, or a condensed ring of a combination of two or more of the foregoing groups, but the embodiments of the present disclosure are not limited thereto.

[0042] If no specific definition is otherwise provided (eg, when no specific definition is otherwise provided), the term "combination" as utilized herein means mixing or copolymerizing.

[0043] In the related art, an aqueous phosphoric acid solution heated to a high temperature has been used as an etching solution to remove a silicon nitride layer pattern formed on a substrate during a semiconductor manufacturing process. However, if such an etchant is used as is, not only the silicon nitride layer is etched, but also the silicon oxide layer is etched, which has the difficulty and / or problem of failing to satisfy the desired or required silicon nitride layer / silicon oxide layer selectivity ratio in the process. In order to solve the above-mentioned difficulties and problems, one or more additives suitable for use with phosphoric acid are being actively studied.

[0044] In order to increase the etching selectivity of the silicon nitride layer to the silicon oxide layer, a silane compound can be used together with a phosphoric acid solution. If a silane compound is included in the etching composition for the silicon nitride layer, the etching selectivity can be improved. However, if the content (e.g., amount) of the silane compound increases, bubbles may be generated due to physical friction, which may be disadvantageous in terms of etching process efficiency. Therefore, it is desirable or necessary to include a silane compound in the etching composition for the silicon nitride layer to improve the etching selectivity, while suppressing or reducing the generation of bubbles or quickly removing the generated bubbles.

[0045] According to one or more embodiments of the present disclosure, the etching composition for a silicon nitride layer may include phosphoric acid, a compound represented by Chemical Formula 1, a compound represented by Chemical Formula 2, and water, wherein the etching composition includes about 11 wt % to about 16 wt % of water based on the total weight of the etching composition, and in the H-NMR spectrum, the Si-OR a (where R a The ratio of the area of ​​the peak derived from Si-CH3 to the area of ​​the peak derived from Si-CH3 is about 2 to about 16:

[0046] Chemical formula 1

[0047] (R 1 ) a (R 2 ) b (CH3)Si-(OR 3 ) (3-a-b) ,

[0048] In Chemical Formula 1,

[0049] R 1 and R 2 may be independently hydrogen, deuterium or a substituted or unsubstituted C1 to C10 alkyl group, R 3 may be a substituted or unsubstituted C1 to C10 alkyl group,

[0050] a and b may each independently be an integer from 0 to 2, and 0≤a+b≤2;

[0051] Chemical formula 2

[0052] (R 5 ) c (R 6 ) d (R 7 )Si-(OR 8 ) (3-c-d) ,

[0053] In chemical formula 2,

[0054] R 5 and R6 can be independently hydrogen, deuterium, C1 to C10 alkyl, one or more hydrogen atoms are replaced by -NR c R d or a C1 to C10 alkyl group, or a C2 to C10 alkyl group wherein at least one -CH2- in the C2 to C10 alkyl group is replaced by -NR e – the group obtained by substitution,

[0055] R 7 One or more hydrogens may be -NR c R d or a C1 to C10 alkyl group, or a C2 to C10 alkyl group wherein at least one -CH2- in the C2 to C10 alkyl group is replaced by -NR e – the group obtained by substitution,

[0056] R c To R e may each independently be hydrogen, substituted or unsubstituted C1 to C5 alkyl, substituted or unsubstituted C3 to C10 cycloalkyl, substituted or unsubstituted C6 to C10 aryl, or a combination thereof (e.g., any suitable combination),

[0057] R 8 may be a substituted or unsubstituted C1 to C10 alkyl group,

[0058] c and d may each independently be one of integers from 0 to 2, and 0≤c+d≤2.

[0059] The etching composition for a silicon nitride layer according to one or more embodiments includes the compound represented by Chemical Formula 1 and the compound represented by Chemical Formula 2, thereby increasing the ratio of the etching rate (etching selectivity) of the silicon nitride layer to the etching rate of the silicon oxide layer and suppressing or reducing abnormal growth of the silicon oxide layer.

[0060] In one or more embodiments, the etching composition concurrently (e.g., simultaneously) satisfies a water content (e.g., amount) and a relative content (e.g., amount) of alkoxysilane relative to alkylsilane within a specific range, thereby suppressing or reducing bubbles generated by friction between the compounds and shortening the time (e.g., duration) desired or required to heat the etching composition to an etching temperature.

[0061] In one or more embodiments, R in Chemical Formula 1 1 To R 3 may be independently a substituted or unsubstituted C1 to C5 alkyl group. For example, in some embodiments, R in Chemical Formula 1 1 To R 3Each of them may independently be a substituted or unsubstituted methyl group, a substituted or unsubstituted ethyl group, or a substituted or unsubstituted propyl group, but the embodiments of the present disclosure are not limited thereto.

[0062] In some embodiments, the sum of a and b in Chemical Formula 1 is 0 or 1 (eg, 0), but the embodiments of the present disclosure are not limited thereto.

[0063] In one or more embodiments, R of Chemical Formula 2 5 To R 7 Each independently may be one or more hydrogen atoms -NR c R d or a C1 to C10 alkyl group, or a C2 to C10 alkyl group wherein at least one -CH2- in the C2 to C10 alkyl group is replaced by -NR e -substituted, or each independently may be, for example, one or more hydrogen atoms are replaced by -NR c R d Substituted C1 to C5 alkyl, or a C2 to C5 alkyl group wherein at least one -CH2- in the C2 to C5 alkyl group is replaced by -NR e - The group obtained by substitution.

[0064] In one or more embodiments, R c To R e Each may independently be hydrogen, substituted or unsubstituted C1 to C5 alkyl, substituted or unsubstituted C6 to C10 aryl, or a combination thereof (e.g., any suitable combination), or for example, hydrogen, substituted or unsubstituted C1 to C5 alkyl, or a combination thereof (e.g., any suitable combination), but the embodiments of the present disclosure are not limited thereto.

[0065] In one or more embodiments, the sum of c and d in Chemical Formula 2 is 0 or 1 (eg, 0), but the embodiments of the present disclosure are not limited thereto.

[0066] In one or more embodiments, in the H-NMR spectrum, the a (where R a The ratio of the area of ​​the peak derived from Si-CH3 to the area of ​​the peak derived from Si-CH3 may be from about 2 to about 16, such as from about 3 to about 16, such as from about 4 to about 16, such as from about 4 to about 15, such as from about 4 to about 14, such as from about 4 to about 13, such as from about 4 to about 12, such as from about 4 to about 11, or such as from about 4 to about 10, but the embodiments of the present disclosure are not limited thereto. a Within the range of the ratio of the area of ​​the peak derived from Si—CH 3 to the area of ​​the peak derived from Si—CH 3 , bubbles generated due to friction between compounds can be suppressed or reduced, and the desired or required time for heating the etching composition to the etching temperature can be shortened.

[0067] In one or more embodiments, the water content (e.g., amount) (e.g., the amount of water) is about 11 wt % to about 16 wt %, such as about 11.5 wt % to about 15 wt %, such as about 12 wt % to about 15 wt %, such as about 12 wt % to about 14.5 wt %, such as about 12 wt % to about 14 wt %, such as about 12 wt % to about 13.8 wt %, such as about 12 wt % to about 13.5 wt %, or such as about 12 wt % to about 13 wt %, based on the total weight of the etching composition, but the embodiments of the present disclosure are not limited thereto. By including water within the above range in the etching composition, bubbles generated due to friction between compounds can be suppressed or reduced, and the time desired or required for heating the etching composition to the etching temperature can be shortened.

[0068] The peak area ratio of the H-NMR spectrum and the water content (eg, amount) in the etching composition concurrently (eg, simultaneously) satisfy the above ranges, so that the beneficial effects of the etching composition according to one or more embodiments can be maximized or increased.

[0069] In one or more embodiments, the content (e.g., amount) of the compound represented by Chemical Formula 1 may be about 0.3 wt % to about 10 wt %, such as about 0.5 wt % to about 10 wt %, such as about 1 wt % to about 10 wt %, such as about 2 wt % to about 10 wt %, such as about 3 wt % to about 10 wt %, such as about 3 wt % to about 9 wt %, or such as about 3 wt % to about 8 wt %, based on the total weight of the etching composition, but the embodiments of the present disclosure are not limited thereto. By including the compound represented by Chemical Formula 1 within the above range in the etching composition, the etching selectivity can be improved or optimized.

[0070] In one or more embodiments, the content (e.g., amount) of the compound represented by Chemical Formula 2 may be about 0.5 wt % to about 30 wt %, such as about 0.5 wt % to about 25 wt %, such as about 0.5 wt % to about 20 wt %, such as about 1 wt % to about 30 wt %, such as about 1 wt % to about 25 wt %, such as about 1 wt % to about 20 wt %, or such as about 1 wt % to about 15 wt %, based on the total weight of the etching composition, but the embodiments of the present disclosure are not limited thereto. By including the compound represented by Chemical Formula 2 within the above range in the etching composition, the etching selectivity can be improved or optimized while suppressing or reducing the abnormal growth of the silicon oxide layer.

[0071] According to one or more embodiments, an etching method performed using an etching composition for a silicon nitride layer is provided.

[0072] The etching method may include, for example, contacting the etching composition for a silicon nitride layer according to one or more embodiments with a substrate having the silicon nitride layer formed thereon.

[0073] The method may further include removing the etching composition for the silicon nitride layer after the contacting.

[0074] The substrate having the silicon nitride layer formed thereon may further include a silicon oxide layer.

[0075] For example, the substrate is not particularly limited as long as the substrate is utilized in the art, and the substrate may be, for example, a semiconductor wafer.

[0076] The contacting of the etching composition for the silicon nitride layer with the substrate having the silicon nitride layer formed thereon may include immersing the substrate having the silicon nitride layer formed thereon in an etching bath containing the etching composition for the silicon nitride layer, or spraying the etching composition for the silicon nitride layer on the substrate having the silicon nitride layer formed thereon, but the embodiments of the present disclosure are not limited thereto.

[0077] In some embodiments, before the etching composition for the silicon nitride layer is contacted with the substrate on which the silicon nitride layer is formed, the etching composition for the silicon nitride layer may be further heated. The etching composition for the silicon nitride layer may be heated to a temperature of about 100° C. or greater than 100° C. (e.g., about 100° C. to about 500° C.). For example, in some embodiments, the etching composition for the silicon nitride layer may be heated to a temperature of about 150° C. to about 300° C., but the embodiments of the present disclosure are not limited thereto.

[0078] By using the etching composition for a silicon nitride layer according to one or more embodiments, the time taken to heat the etching composition to the above-mentioned temperature in the operation of heating the etching composition may be shortened.

[0079] In one or more embodiments, the method may further include drying the substrate from which the silicon nitride layer has been removed after removing the etching composition for the silicon nitride layer.

[0080] If a substrate including a silicon nitride layer and a silicon oxide layer is etched using an etching composition for a silicon nitride layer according to one or more embodiments (for example, when a substrate including a silicon nitride layer and a silicon oxide layer is etched using the etching composition), the etching composition can improve the etching selectivity of the silicon nitride layer relative to the silicon oxide layer and prevent or reduce abnormal growth of silicon oxide.

[0081] Hereinafter, the present disclosure will be described in more detail by way of examples of the above-mentioned etching composition for silicon nitride layer. However, the present disclosure is not technically limited by the following examples.

[0082] Preparation of etching composition for silicon nitride layer

[0083] Example 1 to Example 10

[0084] Methyltrimethoxysilane (alkoxysilane) and 3-aminopropyltriethoxysilane (aminosilane) were dissolved in deionized water (DIW), and the solution was treated under reduced pressure to reduce the alkoxy concentration. Subsequently, phosphoric acid was mixed with the solution to prepare an etching composition for a silicon nitride layer according to each example. Table 1 shows the specific contents of deionized water, alkoxysilane, aminosilane and phosphoric acid, and also shows 1 Si-OR in H-NMR a (where R a is the ratio of the area of ​​the peak derived from substituted or unsubstituted alkyl) to the area of ​​the peak derived from Si-CH3. Figure 1 The etching composition for silicon nitride layer according to Example 1 is shown in 1 H-NMR spectrum.

[0085] 1 The measurement conditions of H-NMR are as follows. The chemical shift of the peak derived from Si-CH3 appears at 0.2 parts per million (ppm), while that derived from Si-OR a The chemical shifts of the peaks appeared at 3.8 ppm, 3.5 ppm, 3.4 ppm, 3.2 ppm, and 0.9 ppm.

[0086] < 1 H-NMR measurement conditions>

[0087] NMR apparatus: AVANCE III 300 (Bruker Corporation)

[0088] Resonance frequency: 300 MHz

[0089] Total: 16 times

[0090] Measuring solvent: CDCl3

[0091] Reference material and chemical shift of reference peak: Tetramethyl silane (TMS), 0 ppm

[0092] Sample concentration: [CDCl3: sample = 1:1]

[0093] Comparative Examples 1 to 4

[0094] The etching composition of Comparative Example 1 is a phosphoric acid aqueous solution, and the etching compositions of Comparative Examples 2 to 4 include phosphoric acid, alkoxysilane, aminosilane, and DIW in the amounts shown in Table 1.

[0095] Table 1

[0096]

[0097] Assessment 1: Assessment of Bubble Volume Reduction

[0098] Each 15g of each of the etching compositions of Comparative Example 1 to Comparative Example 4 and Example 1 to Example 10 is put into a 20mL vial and shaken 40 times, and then placed on a base plate (e.g., plate or platform) with text to check text. When the etching composition is shaken, bubbles are produced in the etching composition by physical friction, and then the degree of bubble retention over time, i.e. the degree of text visibility, is observed, to assess the degree of bubble removal. Result is shown in Table 2. In Table 2, "○" represents that text is clearly distinguished because there is no bubble or there is a small amount of bubble, "△" represents that text is partially distinguished because there is a certain amount of bubble, and "X" represents that text is not distinguished because there is a large amount of bubbles or solution is frozen.

[0099] Table 2

[0100] 0 minutes 1 minute 2 minutes 3 minutes 4 minutes 5 minutes Comparative Example 1 ○ ○ ○ ○ ○ ○ Comparative Example 2 X X X X X △ Comparative Example 3 X X X X X X Comparative Example 4 X X X X X X Example 1 ○ ○ ○ ○ ○ ○ Example 2 △ △ △ ○ ○ ○ Example 3 △ △ △ ○ ○ ○ Example 4 X △ △ ○ ○ ○ Example 5 X △ △ △ ○ ○ Example 6 ○ ○ ○ ○ ○ ○ Example 7 ○ ○ ○ ○ ○ ○ Example 8 △ ○ ○ ○ ○ ○ Example 9 △ △ ○ ○ ○ ○ Example 10 X X △ ○ ○ ○

[0101] Referring to Table 2, each of the etching compositions of Examples 1 to 9 exhibited no bubbles or a small amount of bubbles, wherein if bubbles were generated, the bubbles would decrease or disappear within 1 minute. In contrast, each of the etching compositions of the comparative examples exhibited a large amount of bubbles or crystallization. The composition of Comparative Example 4 exhibited agglomeration of the silane compound.

[0102] Assessment 2: Etch rate, etch selectivity, and etch byproducts

[0103] Each of the etching compositions for silicon nitride layers according to Examples 1 to 10 and Comparative Examples 1 to 4 was put into a beaker and heated to an etching temperature of 165° C., and then a silicon nitride layer (LP-SiN layer) or a silicon oxide layer (PE-SiO layer) was added thereto, and then etching was performed at the etching temperature for 30 minutes. Before and after etching, the thickness of the LP-SiN layer or the PE-SiO layer was measured by using an ellipsometer to obtain an etching rate. The etching rate ratio (etching selectivity=A / B) was calculated using the etching rate (A) of the silicon nitride layer and the etching rate (B) of the silicon oxide layer, and in addition, the presence or absence of byproducts after etching was checked with the naked eye, and the results are shown in Table 3.

[0104] Table 3

[0105]

[0106] Referring to Table 3, each of the compositions of the examples exhibits excellent or appropriate etching rate and etching selectivity, and no by-products are present after the etching process.

[0107] In the present disclosure, the terms “comprise(s) / comprising”, “include(s) / including” or “have(has) / having)” are intended to specify the presence of implemented characteristics, numbers, steps, constituent elements or combinations thereof, but it should be understood that the possibility of the presence or addition of one or more other characteristics, numbers, steps, constituent elements or combinations is not excluded in advance.

[0108] Unless the context clearly indicates otherwise, the singular forms "a / an" and "the" used in this article are also intended to include plural forms. In addition, when describing the embodiments of the present disclosure, "may" is used to refer to "one or more embodiments of the present disclosure". When expressions such as "at least one of...", "one of..." and "selected from..." appear before a series of elements, it is to modify the elements of the entire series rather than modifying the individual elements in the series. For example, "at least one of a, b or c", "at least one of a, b and / or c", "selected from a, b and c", "selected from at least one of a to c", etc. can mean only including a, only including b, only including c, including (for example, including) both a and b, including (for example, including) both a and c, including (for example, including) both b and c, including all a, b and c or their variants. In addition, the " / " used in this article can be interpreted as "and" or "or" as appropriate.

[0109] As used herein, the terms "substantially," "about," and similar terms are used as terms of approximation rather than degree, and are intended to account for the inherent deviations in measured or calculated values ​​that one of ordinary skill in the art would recognize. As used herein, "about" or "approximately" also includes the stated value and means within an acceptable range of deviation for the particular value as determined by one of ordinary skill in the art, taking into account the measurement in question and the errors associated with the measurement of a particular quantity (i.e., the limitations of the measurement system). For example, "about" may mean within one or more standard deviations, or within ±30%, 20%, 10%, 5% of the stated value.

[0110] Any numerical range described herein is intended to include all sub-ranges of the same numerical precision that fall within the range. For example, the range of "1.0 to 10.0" is intended to include all sub-ranges between (and including) the minimum value 1.0 and the maximum value 10.0, i.e., having a minimum value equal to or greater than 1.0 and a maximum value equal to or less than 10.0, such as (for example) 2.4 to 7.6. Any maximum numerical limit described herein is intended to include all lower numerical limits that fall within it, and any minimum numerical limit described in this specification is intended to include all higher numerical limits that fall within it. Therefore, the applicant reserves the right to amend this specification (including the claims) to explicitly state any sub-ranges that fall within the range explicitly stated herein.

[0111] In the above, certain embodiments of the present disclosure have been described and illustrated. However, it is obvious to those skilled in the art that the present disclosure is not limited to the described embodiments, but various modifications and changes can be made without departing from the spirit and scope of the present disclosure. Therefore, the modified or changed embodiments themselves may not be understood separately from the technical ideas and aspects of the present disclosure, and the modified embodiments are within the scope of the claims of the present disclosure and their equivalent forms.

Claims

1. An etching composition comprising: Phosphoric acid; A compound represented by Chemical Formula 1; a compound represented by Chemical Formula 2; and water, wherein the etching composition comprises 11 wt % to 16 wt % of water, based on the total weight of the etching composition, and In the proton nuclear magnetic resonance spectrum of the etching composition, the a The ratio of the area of ​​the peak derived from Si-CH3 to the area of ​​the peak derived from Si-CH3 is 2 to 16, wherein R a is a substituted or unsubstituted alkyl group: Chemical formula 1 (R 1 ) a (R 2 ) b (CH3)Si-(OR 3 ) (3-a-b) , In Chemical Formula 1, R 1 and R 2 are each independently hydrogen, deuterium or a substituted or unsubstituted C1 to C10 alkyl group, R 3 are each independently a substituted or unsubstituted C1 to C10 alkyl group, a and b are each independently an integer from 0 to 2, and 0≤a+b≤2; Chemical formula 2 (R 5 ) c (R 6 ) d (R 7 )Si-(OR 8 ) (3-c-d) , In chemical formula 2, R 5 and R 6 are each independently hydrogen, deuterium, C1 to C10 alkyl, one or more hydrogen atoms are replaced by -NR c R d or a C1 to C10 alkyl group, or a C2 to C10 alkyl group wherein at least one -CH2- in the C2 to C10 alkyl group is replaced by -NR e – the group obtained by substitution, R 7 One or more hydrogens are c R d or a C1 to C10 alkyl group, or a C2 to C10 alkyl group wherein at least one -CH2- in the C2 to C10 alkyl group is replaced by -NRe – the group obtained by substitution, R c To R e are each independently hydrogen, substituted or unsubstituted C1 to C5 alkyl, substituted or unsubstituted C3 to C10 cycloalkyl, substituted or unsubstituted C6 to C10 aryl, or a combination thereof, R 8 is a substituted or unsubstituted C1 to C10 alkyl group, c and d are each independently an integer from 0 to 2, and 0≤c+d≤2, and The etching composition is used for silicon nitride layer.

2. The etching composition according to claim 1, wherein in Chemical Formula 1, R 1 To R 3 Each is independently a substituted or unsubstituted C1 to C5 alkyl group.

3. The etching composition according to claim 1, wherein in Chemical Formula 1, R 3 It is methyl, ethyl or propyl. The etching composition according to claim 1 , wherein in Chemical Formula 1, a+b is 0.

5. The etching composition according to claim 1, wherein in Chemical Formula 2, R 5 To R 7 Each independently is one or more of the hydrogen atoms -NR c R d or a C1 to C10 alkyl group, or a C2 to C10 alkyl group wherein at least one -CH2- in the C2 to C10 alkyl group is replaced by -NR e - The group obtained by substitution.

6. The etching composition according to claim 5, wherein R c To R e Each is independently hydrogen, substituted or unsubstituted C1 to C5 alkyl, or a combination thereof. 7 . The etching composition according to claim 1 , wherein in Chemical Formula 2, c+d is 0.

8. The etching composition according to claim 1, wherein the amount of water is 12 wt% to 15 wt% based on the total weight of the etching composition.

9. The etching composition according to claim 1, wherein the a The ratio of the area of ​​the peak of to the area of ​​the peak derived from Si-CH3 is 2 to 10, wherein R a is a substituted or unsubstituted alkyl group. 10 . The etching composition according to claim 1 , wherein an amount of the compound represented by Chemical Formula 1 is 0.3 wt % to 10 wt % based on the total weight of the etching composition. 11 . The etching composition according to claim 1 , wherein an amount of the compound represented by Chemical Formula 2 is 0.5 wt % to 30 wt % based on the total weight of the etching composition.

12. A method for etching a silicon nitride layer, comprising: The surface of the silicon nitride layer is contacted with the etching composition of claim 1.

13. A silicon nitride layer, comprising: An etched surface etched by the etching composition according to claim 1.