Beautifying agent for high-early-strength easy-to-demould concrete and preparation method of beautifying agent
Through the combination of emulsifier and capsule coating hydration accelerator, the problems of low appearance and demolding efficiency of concrete surface are solved, and concrete beautifiers with high early strength and easy demolding are realized, reducing bubbles and color difference, and improving the interface Strength and productivity.
Patent Information
- Application Number
- CN202411427934.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-26
AI Technical Summary
The surface of existing concrete is poorly beautiful, and oily and water-based isolators have problems such as large oil film thickness, difficult to eliminate bubbles, low surface strength and serious color difference, which is difficult to meet the construction industry's demand for early strength and mold release cycle.
Using a combination of emulsifier, base oil, capsule coated hydration accelerator and defoaming agent, a thin oil film is formed through emulsification system stability and phacoemulsification technology, which promotes hydration and defoaming, and improves interface strength and mold release efficiency.
The concrete surface color difference, bubble reduction, and interface strength improvement are achieved, which shortens the demolding time and improves production efficiency and surface aesthetics.
Smart Images

Figure BDA0005082705390000071 
Figure BDA0005082705390000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building material chemistry, and particularly relates to a beautifying agent for high-early-strength and easy-to-release concrete and a preparation method thereof. Background Art
[0002] With the rapid development of the construction industry, in addition to meeting the basic working performance, mechanical properties and durability of concrete, higher requirements are placed on the surface aesthetics of concrete. For concrete using formwork, an isolating agent is usually applied to the interface of the formwork. Currently, the commonly used isolating agents on the market are mainly oily and water-based. In the early days, the problem of concrete surface beautification was not considered. In order to reduce the interfacial adhesion between concrete and the formwork, engine oil or waste engine oil was usually used and applied to the inner wall of the formwork for lubrication and isolation. However, when oil is used as an isolating agent, there is a high viscosity on the surface of the oil film, bubbles are difficult to remove, oil stains are serious, the color of the concrete surface is uneven, and the aesthetics of the concrete cannot meet current needs. The water-based isolating agent is mainly due to the small thickness of the oil film and poor wettability. At the same time, due to internal vibration, the water-cement ratio of the formwork interface will increase, the surface strength will be low, the sticking phenomenon will be serious, and the surface color difference will be serious due to uneven hydration.
[0003] The art is in urgent need of a beautifying agent for high early strength and easy demoulding concrete. Summary of the invention
[0004] The purpose of the present invention is to provide a beautifier for high early strength and easy demoulding concrete and a preparation method thereof to solve the problems existing in the above-mentioned prior art. The preparation of a beautifier for high early strength and easy demoulding concrete is a trend to solve the current concrete surface problems, and is particularly suitable for construction sites with short demoulding cycles and high requirements for surface color difference, bubbles, and surface strength.
[0005] One of the technical solutions provided by the present invention:
[0006] A beautifier for high-early-strength and easy-to-release concrete is prepared by emulsifying the following raw materials, calculated by weight: 50-200‰ of emulsifier, 300-400‰ of base oil, 110-200‰ of capsule-coated hydration promoter and 5-10‰ of defoamer, and the rest is water; the emulsifier is a mixture of anionic emulsifier and nonionic emulsifier; the base oil is a mixture of vegetable oil and mineral oil.
[0007] Preferably, the mass ratio of the anionic emulsifier to the nonionic emulsifier is 3:(8-10).
[0008] More preferably, the anionic emulsifier is selected from sodium oleate, potassium oleate, sodium stearate or potassium stearate; the nonionic emulsifier is selected from OP-10, OP-20, OP-30, TW-20, TW-40 or TW-60.
[0009] Preferably, the base oil is a mixture of vegetable oil and mineral oil, and the mass ratio of the vegetable oil to the mineral oil is 1:(1.25-3).
[0010] More preferably, the vegetable oil is selected from soybean oil, rapeseed oil or corn oil; and the mineral oil is selected from low-viscosity hydrogenated mineral oil 60N or 100N.
[0011] Preferably, the defoamer is selected from acetylene glycol defoamers, polyether-modified silicone defoamers or silicone defoamers.
[0012] Preferably, the method for preparing the capsule-coated hydration promoter comprises the following steps:
[0013] The hydration promoter is dissolved in deionized water, the temperature is raised to 30-40°C, and an initiator is added at the same time, stirred and dissolved to prepare an aqueous solution A; an alkyl acrylic monomer, a cross-linking monomer and an emulsifier are prepared to prepare an oil solution B; the oil solution B is added to the aqueous solution A, ultrasonically emulsified to obtain a water / oil emulsion, and the water / oil emulsion is stirred and heated to react under a N2 atmosphere to prepare the capsule-coated hydration promoter.
[0014] More preferably, the hydration promoter is selected from aluminum sulfate or sodium aluminate; the initiator is ammonium cerium nitrate or ammonium cerium sulfate; the alkyl acrylic anhydride monomer is one or a mixture of acrylic anhydride, methacrylic anhydride, methyl methacrylate and ethyl methacrylate; the cross-linking monomer is 1,4-butanediol dimethacrylate, 1,4-butanediol diacrylate, 1,3-butanediol dimethacrylate, 1,3-butanediol diacrylate, ethylene glycol dimethacrylate, ethylene glycol diacrylate, 1,3-propylene glycol dimethacrylate or 1,3-propylene glycol diacrylate; and the emulsifier in the preparation of the capsule-coated hydration promoter is a mixture of Span-20 and Tween-80.
[0015] More preferably, the mass ratio of the hydration accelerator, deionized water and initiator is (20-40): (60-80): (0.8-1.5); the mass ratio of the alkyl acrylic monomer, the cross-linking monomer and the emulsifier is (20-40): 1: (8-12); the rate of the ultrasonic emulsification is 8000-10000 r / min, the time is 20-30 min, the temperature of the heating reaction is 40-50°C, and the time is 1-2 h.
[0016] The second technical solution provided by the present invention is:
[0017] A method for preparing the above-mentioned beautifier for high early strength and easy demoulding concrete comprises the following steps: weighing raw materials, mixing vegetable oil, mineral oil, anionic emulsifier and nonionic emulsifier, stirring and mixing at room temperature, then dripping capsule-coated hydration promoter at a uniform speed, and finally adding defoamer, adding water, and continuing stirring to prepare the beautifier for high early strength and easy demoulding concrete.
[0018] Preferably, the mixing and stirring speed is 1000-2000r / min.
[0019] Technical principle of the present invention: The present invention can make the water-in-oil emulsion system more stable, the emulsion particle size smaller, the oil film thickness thinner, the interfacial viscosity lower, and the bubbles easier to remove through the joint action of non-ionic and anionic emulsifiers. The joint action of vegetable oil and mineral oil can make it oriented at the interface. The carboxyl group in the vegetable oil can react with the calcium in the slurry to form calcium soap. The carboxyl head end is more slurry-friendly, and the alkyl end forms a hydrophobic interface with the mineral oil and is more template-friendly. During the pouring process, the bubbles at the interface between the template and the slurry can be quickly eliminated by vibration and defoaming agent. As the hydration proceeds, the capsule-coated hydration promoter is quickly hydrolyzed to release the hydration promoter, the interface strength rises rapidly, the bubbles in the concrete are blocked from moving at the interface, and new bubbles will not move to the interface, which greatly reduces the amount of bubbles at the interface. At the same time, due to the rapid hydration of the interface slurry and the rapid improvement of the interface strength, the demoulding time can be greatly shortened and the production efficiency can be improved. During the vibration process, the aqueous solution migrates to the interface, causing a large difference in the water-binder ratio of the interface slurry, which can also cause color difference problems on the concrete surface. The rapid hydration in the present invention can also avoid the color difference problem caused by hydration differences.
[0020] Compared with the prior art, the present invention has the following advantages and technical effects:
[0021] The beautifier for high early strength and easy demoulding concrete provided by the present invention has the performance of improving the early strength of the concrete interface, reducing the viscose performance, and improving the surface rebound strength. It is a concrete beautifier that can solve the problems of uneven color difference and many bubbles on the concrete surface.
[0022] The beautifier for high early strength easy demoulding concrete provided by the present invention can be applied to various formwork concretes, and is particularly suitable for construction sites with short demoulding cycles and high requirements on surface color difference, bubbles and surface strength. DETAILED DESCRIPTION
[0023] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0024] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0025] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0026] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0027] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0028] The normal temperature of the present invention refers to 25±2°C.
[0029] In the embodiments of the present invention, “parts” refer to “parts by mass” unless otherwise specified.
[0030] Example 1 Preparation method of a beautifying agent for high early strength and easy demoulding concrete
[0031] (1) Weigh 20 parts of aluminum sulfate and dissolve it in 60 parts of deionized water, raise the temperature to 30° C., and simultaneously add 1 part of ammonium cerium nitrate, stir and dissolve to prepare an aqueous solution A; weigh 25 parts of ethyl methacrylate monomer, 1 part of 1,4-butanediol dimethacrylate, 5 parts of Span-20 and 5 parts of Tween-80 to prepare an oil solution B; add the oil solution B to the aqueous solution A, emulsify for 20 minutes under ultrasonic dispersion (at a rate of 8000 r / min) to obtain a water / oil emulsion; stir and heat the water / oil emulsion under a N2 atmosphere, raise the temperature to 40° C. and react for 1 hour to obtain a capsule-coated hydration promoter.
[0032] (2) Into a three-necked flask equipped with a stirrer, 100 parts of soybean oil, 250 parts of 60N, 15 parts of sodium oleate, and 50 parts of OP-10 were added in sequence, and stirred at a high speed of 1000 / min at room temperature for 10 minutes. Then, the capsule-coated hydration promoter prepared in step (1) was uniformly added dropwise into the three-necked flask for 30 minutes. Finally, 8 parts of acetylene glycol defoamer were added, and water was added to make the total weight portion 1000 parts, and stirring was continued for 10 minutes to prepare a beautifier for high early strength and easy demoulding concrete.
[0033] Example 2 Preparation method of a beautifying agent for high early strength and easy demoulding concrete
[0034] (1) Weigh 30 parts of sodium aluminum aluminate and dissolve them in 70 parts of deionized water, heat them to 35° C., and simultaneously add 1.2 parts of ammonium cerium sulfate, stir and dissolve them to prepare an aqueous solution A; weigh 30 parts of methacrylic anhydride monomer, 1.5 parts of 1,3-butanediol diacrylate, 6 parts of Span-20 and 6 parts of Tween-80 to prepare an oil solution B, add the oil solution B to the aqueous solution A, and emulsify for 25 minutes under ultrasonic dispersion (at a rate of 10000 r / min) to obtain a water / oil emulsion; stir and heat the water / oil emulsion under a N2 atmosphere, heat it to 45° C. and react for 2 hours to obtain a capsule-coated hydration promoter;
[0035] (2) Into a three-necked flask equipped with a stirrer, 150 parts of soybean oil, 300 parts of 100N, 25 parts of potassium oleate, and 80 parts of TW-20 were added in sequence, and stirred at a high speed of 1500 / min at room temperature for 20 minutes. Then, the capsule-coated hydration promoter prepared in step (1) was uniformly added dropwise to the three-necked flask for 40 minutes. Finally, 5 parts of a polyether-modified silicone defoamer was added, and water was added to make the total weight portion 1000 parts, and stirring was continued for 10 minutes to prepare a beautifier for high early strength and easy demoulding concrete.
[0036] Example 3 Preparation method of a beautifying agent for high early strength and easy demoulding concrete
[0037] (1) Weigh 40 parts of aluminum sulfate and dissolve it in 80 parts of deionized water, raise the temperature to 40° C., and add 0.8 parts of ammonium cerium nitrate at the same time, stir and dissolve to prepare an aqueous solution A; weigh 40 parts of methyl methacrylate monomer, 1 part of 1,3-propylene glycol diacrylate, 4 parts of Span-20 and 8 parts of Tween-80 to prepare an oil solution B; add the oil solution B to the aqueous solution A, emulsify for 30 minutes under ultrasonic dispersion (speed of 9000 r / min) to obtain a water / oil emulsion; stir and heat the water / oil emulsion under a N2 atmosphere, raise the temperature to 50° C. and react for 2 hours to obtain a capsule-coated hydration promoter;
[0038] (2) Into a three-necked flask equipped with a stirrer, 200 parts of corn oil, 250 parts of 60N, 30 parts of potassium stearate, and 100 parts of TW-40 were added in sequence, and stirred at a high speed of 2000 r / min at room temperature for 20 minutes. Then, the capsule-coated hydration promoter prepared in step (1) was uniformly added dropwise to the three-necked flask for 50 minutes. Finally, 6 parts of an organosilicon defoamer were added, and water was added to make the total weight portion 1000 parts, and stirring was continued for 10 minutes to prepare a beautifier for high early strength and easy demoulding concrete.
[0039] Example 4 Preparation method of a beautifying agent for high early strength and easy demoulding concrete
[0040] (1) Weigh 30 parts of sodium aluminate and dissolve it in 70 parts of deionized water, raise the temperature to 40° C., and simultaneously add 1.3 parts of ammonium cerium sulfate, stir and dissolve to prepare an aqueous solution A; weigh 30 parts of acrylic anhydride monomer, 1.3 parts of 1,4-butanediol diacrylate, 3 parts of Span-20 and 7 parts of Tween-80 to prepare an oil solution B; add the oil solution B to the aqueous solution A, emulsify for 25 minutes under ultrasonic dispersion (at a rate of 8000 r / min) to obtain a water / oil emulsion; stir and heat the water / oil emulsion under a N2 atmosphere, raise the temperature to 40° C. and react for 1.5 hours to obtain a capsule-coated hydration promoter;
[0041] (2) 150 parts of rapeseed oil, 300 parts of 100N, 30 parts of sodium stearate, and 80 parts of OP-20 were added to a three-necked flask equipped with a stirrer, and stirred at a high speed of 1000 r / min at room temperature for 30 minutes. Then, the capsule-coated hydration promoter prepared in step (1) was uniformly added dropwise to the three-necked flask for 50 minutes. Finally, 7 parts of polyether-modified silicone defoamer were added, and water was added to make the total mass part 1000 parts, and stirring was continued for 10 minutes to prepare a beautifier for high early strength and easy demoulding concrete.
[0042] Comparative Example 1
[0043] The same as Example 1, except that the encapsulated hydration promoter was not added, and the encapsulated hydration promoter was replaced by an equal mass portion of water.
[0044] Comparative Example 2
[0045] Same as Example 1, except that vegetable oil (soybean oil) was not added and was replaced by an equal mass portion of water.
[0046] Comparative Example 3
[0047] The same as Example 1, except that no defoamer (acetylene glycol defoamer) was added, and the defoamer was replaced by an equal mass portion of water.
[0048] Comparative Example 4
[0049] The same as Example 1, except that no anionic emulsifier (sodium oleate) was added, and the anionic emulsifier was replaced by an equal mass portion of water.
[0050] Effect verification:
[0051] The test was conducted in accordance with JC / T949-2005 "Release Agents for Concrete Products" to measure the stability, adhesion, demoulding time and appearance of the test pieces after demoulding of Examples 1-4 and Comparative Examples 1-4. The specific results are shown in Table 1.
[0052] Table 1
[0053]
[0054]
[0055] The beautifier for high early strength and easy demoulding concrete prepared in Examples 1-4 of the present invention has a short demoulding time, uniform color difference, and greatly reduced bubble area. In Comparative Example 1, the capsule-coated hydration promoter is removed, which seriously affects the demoulding time and has a large amount of sticky film. After the vegetable oil is removed in Comparative Example 2, it cannot form calcium soap with calcium in the slurry, and the bubble area increases; after the defoamer is removed in Comparative Example 3, the surface bubbles cannot be quickly eliminated, and the bubble area is greatly increased; after the anionic emulsifier is removed in Comparative Example 4, the emulsion stability deteriorates and obvious stratification occurs.
[0056] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A beautifying agent for high early strength and easy demoulding concrete, characterized in that: Calculated by weight, the emulsifier is emulsified from the following raw materials: 50-200‰ emulsifier, 300-400‰ base oil, 110-200‰ capsule-coated hydration promoter and 5-10‰ defoamer, and the rest is water; the emulsifier is a mixture of anionic emulsifier and nonionic emulsifier; the base oil is a mixture of vegetable oil and mineral oil.
2. The beautifying agent for high early strength and easy demoulding concrete according to claim 1, characterized in that: The mass ratio of the anionic emulsifier to the nonionic emulsifier is 3:(8-10).
3. The beautifying agent for high early strength and easy demoulding concrete according to claim 1, characterized in that: The mass ratio of the vegetable oil to the mineral oil is 1:(1.25-3).
4. The beautifying agent for high early strength and easy demoulding concrete according to claim 1, characterized in that: The preparation method of the capsule-coated hydration promoter comprises the following steps: Dissolve the hydration accelerator in deionized water, raise the temperature to 30-40°C, add the initiator, stir and dissolve, and prepare aqueous solution A; The alkyl acrylic monomer, the cross-linking monomer and the emulsifier are prepared into an oil phase solution B; The oil phase solution B is added to the water phase solution A, and ultrasonic emulsification is performed to obtain a water / oil emulsion. The water / oil emulsion is stirred and heated for reaction under a N2 atmosphere to prepare the capsule-coated hydration promoter.
5. The beautifying agent for high early strength and easy demoulding concrete according to claim 4, characterized in that: The hydration accelerator is selected from aluminum sulfate or sodium aluminate.
6. The beautifying agent for high early strength and easy demoulding concrete according to claim 4, characterized in that: The mass ratio of the hydration accelerator, deionized water and initiator is (20-40): (60-80): (0.8-1.5).
7. The beautifying agent for high early strength and easy demoulding concrete according to claim 4, characterized in that: The mass ratio of the alkyl acrylic monomer, the cross-linking monomer and the emulsifier is (20-40):1:(8-12).
8. The beautifying agent for high early strength and easy demoulding concrete according to claim 4, characterized in that: The heating reaction is carried out at a temperature of 40-50°C and for a time of 1-2 hours.
9. A method for preparing the beautifying agent for high early strength and easy demoulding concrete according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: weighing raw materials, mixing vegetable oil, mineral oil, anionic emulsifier and nonionic emulsifier, stirring and mixing at room temperature, then dripping capsule-coated hydration promoter at a uniform speed, and finally adding defoamer, adding water, and continuing stirring to prepare the beautifier for high early strength and easy demoulding concrete.