Low-metal-corrosion chip post-CMP cleaning solution, and preparation method and application of low-metal-corrosion chip post-CMP cleaning solution

By using amino compounds, chelating agents, and pH adjusters in the post-CMP cleaning solution, the metal corrosion problem caused by the post-CMP cleaning solution was solved, resulting in better cleaning performance and chip performance.

CN119020119APending Publication Date: 2024-11-26ZHEJIANG AUFIRST MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411089302.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing CMP post-cleaning solutions are prone to causing metal corrosion during the cleaning process, affecting chip performance and yield.

Method used

A low-metal corrosion chip CMP post-cleaning solution containing amino compounds, chelating agents, and pH adjusters is used. The amino compounds form a passivation film on the copper surface, the chelating agents complex with copper ions, and the pH adjusters provide a suitable acidic environment to inhibit metal corrosion.

Benefits of technology

It effectively inhibits metal corrosion, improves cleaning effect, ensures smooth and low-corrosion chip surface, and improves chip performance and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020119A_ABST
    Figure CN119020119A_ABST
Patent Text Reader

Abstract

The invention provides a low-metal-corrosion chip post-CMP cleaning solution and a preparation method and application thereof. The low-metal-corrosion chip post-CMP cleaning solution comprises the following components in parts by weight: 15-30 parts of an amino compound; 10-30 parts of a chelating agent; 0.001 to 5 parts of a pH regulator; and 70-95 parts of ultrapure water. The low-metal-corrosion chip post-CMP cleaning solution is acidic. The invention further discloses a preparation method and application of the low-metal-corrosion chip post-CMP cleaning solution. The low-metal-corrosion chip post-CMP cleaning solution is used for cleaning a semiconductor chip, and the corrosion inhibition effect on Cu can be improved while the cleaning effect is kept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to chip post-CMP cleaning liquid technology, and in particular to a chip post-CMP cleaning liquid with low metal corrosion, and a preparation method and application thereof. Background Art

[0002] Compared with traditional aluminum wires, copper has the advantages of low resistance and high resistance to point migration. Therefore, copper wiring is widely used in very large-scale integrated circuits. In industry, the dual Damascene process is generally used to prepare copper wiring, and the excess copper generated during the deposition process is removed by chemical mechanical polishing (CMP). Chemical mechanical polishing technology has become the most effective means to achieve global flatness of chips. While performing CMP on the surface of the wafer to achieve high flatness, the polishing liquid usually includes an aqueous solution, a low pH or high pH nanodispersant containing abrasive particles, an oxidant, a hydrogen peroxide decomposition accelerator, and an anti-corrosion additive. Because of this, a large amount of contaminants will remain on the surface of the wafer after CMP, which needs to be removed by post-CMP cleaning.

[0003] With the continuous development of integrated circuits, metal corrosion has become the main defect of post-CMP cleaning, and the effective inhibition of copper corrosion has become the key to improving the post-CMP process performance of copper interconnects. Therefore, the development of new cleaning solutions that effectively control metal corrosion during the post-CMP cleaning process is crucial to improving chip performance and yield. Summary of the invention

[0004] The purpose of the present invention is to propose a chip post-CMP cleaning liquid with low metal corrosion to address the problem that corrosion defects are easily generated during the current post-CMP cleaning. The cleaning liquid is used for cleaning semiconductor chips and can improve the corrosion inhibition effect on Cu while maintaining the cleaning effect.

[0005] It should be noted that, in the present invention, unless otherwise specified, the specific meaning of "including" in relation to composition limitations and descriptions includes both open-ended "including", "comprising", etc. and similar meanings, as well as closed-ended "composed of", "composed of", etc. and similar meanings.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a low metal corrosion chip post-CMP cleaning solution, comprising the following components in weight proportions:

[0007]

[0008] Furthermore, the amino compound is an amino organic urea.

[0009] Furthermore, the amino compound is one or more of 4-carboxyphenylthiourea, semicarbazide, chitosan oligosaccharide semicarbazide Schiff base and L-glucose thiourea.

[0010] Furthermore, the amino compound is preferably a chitosan oligosaccharide thiocarbamide Schiff base.

[0011] The amino compound contains multiple hydrophilic polar groups such as hydroxyl, amino and glycosidic bonds, which improve its own hydrophilicity and water solubility. At the same time, it has strong hydrogen bonding within and between molecules, has a stable rigid structure, further improves the solubility of the compound, and provides a basis for the stability of the subsequent solution system. At the same time, the urea group in the thiourea structure it contains can also interact with the copper surface to form a passivation film on the copper surface, which has good film-forming stability and reduces the contact between the copper surface and the corrosive medium, thereby achieving the effect of inhibiting metal corrosion. In addition, the amino compound can coordinate with the copper ions on the chip surface and the solution system, exist in the form of a stable soluble complex, and be taken away from the chip surface with the flowing cleaning solution to achieve a good cleaning effect.

[0012] The preferred chitosan oligosaccharide aminothiourea Schiff base can be vertically adsorbed on the copper metal surface through the C=N bond in the Schiff base structure, and has an excellent effect of inhibiting metal corrosion on the chip.

[0013] Furthermore, the amino compound is 15-25 parts.

[0014] Furthermore, the chelating agent is an organic phosphine derivative.

[0015] Furthermore, the organic phosphine derivative is one or more of diethyl ((bis(2-hydroxyethyl)amino)methyl)phosphonate, 2-aminoethylphosphonic acid and N,N-bis(phosphinohydroxymethyl)glycine.

[0016] Furthermore, the chelating agent is preferably N,N-bis(phosphinomethyl)glycine.

[0017] The chelating agent of the present invention has the functions of corrosion inhibition and cleaning. The addition of the chelating agent can be used in combination with an amino compound to accelerate the dissolution of the oxide layer on the copper surface, and can be complexed with more copper ions to form a stable complex, thereby improving the cleaning effect of the entire system. At the same time, the molecular structure of the chelating agent has a P heteroatom and a hydrophilic group with strong adsorption capacity, which further enhances the adsorption force of the amino compound on the metal surface, and is easy to form a coordination bond with the copper surface to prevent further oxidation of the copper, and has a better corrosion inhibition effect on the chip, thereby promoting the adsorption of the cleaning solution on the copper surface to slow down the corrosion.

[0018] Furthermore, the chelating agent is 15-22 parts.

[0019] Furthermore, the pH regulator is one or more of DL-malic acid, itaconic acid, gluconic acid, agaric acid and quinic acid.

[0020] Furthermore, the pH regulator is preferably agaricic acid.

[0021] The pH regulator of the present invention can provide a suitable acidic environment to dissolve the oxide layer and other residual pollutants on the copper surface, chelate the copper metal ions in the solution, enhance the cleaning effect, and form a hydrophobic film on the copper surface with a long-chain alkyl group as a hydrophobic branch chain, further enhancing the effect of inhibiting corrosion.

[0022] Furthermore, the low metal corrosion chip post-CMP cleaning solution is acidic with a pH of 2-6.

[0023] Furthermore, the pH of the low metal corrosion chip post-CMP cleaning solution is preferably 2.5-5.5.

[0024] Furthermore, the pH adjuster is 2-5 parts.

[0025] Furthermore, the ultrapure water is 75-85 parts.

[0026] Another object of the present invention is to disclose a method for preparing the low metal corrosion chip post-CMP cleaning solution, comprising the following steps:

[0027] Weigh each component separately, mix and dissolve all the components completely, and then obtain the post-CMP cleaning solution for chips with low metal corrosion.

[0028] Another object of the present invention is to disclose the use of the low metal corrosion chip post-CMP cleaning solution in the field of cleaning semiconductor chips, especially in the field of cleaning semiconductor copper chips. Using the cleaning solution to clean semiconductor chips can effectively inhibit the corrosion of Cu.

[0029] Furthermore, a method for cleaning a semiconductor chip using the low metal corrosion chip post-CMP cleaning solution comprises the following steps:

[0030] Step 1: preparing the low metal corrosion chip post-CMP cleaning solution with ultrapure water into an aqueous solution with a mass concentration of 10-100%, and then using the aqueous solution to soak a semiconductor chip at room temperature to obtain a soaked semiconductor chip;

[0031] Step 2: Rinse the soaked semiconductor chip in ultrapure water to complete the cleaning process of the semiconductor chip.

[0032] Furthermore, in step 1, the low metal corrosion chip post-CMP cleaning solution is prepared into an aqueous solution with a mass concentration of 30-80% using ultrapure water.

[0033] Furthermore, the soaking time in step 1 is 5-30 minutes.

[0034] Furthermore, in step 2, the semiconductor chip after immersion is rinsed in pure water at least twice.

[0035] The low metal corrosion chip post-CMP cleaning solution of the present invention, its preparation method and application have the following advantages compared with the prior art:

[0036] 1) The amino compound of the present invention contains multiple hydrophilic polar groups such as hydroxyl, amino and glycosidic bonds, which improves its own hydrophilicity and water solubility, and at the same time, it has strong hydrogen bonding within and between molecules, has a stable rigid structure, further improves the solubility of the compound, and provides a basis for the stability of the subsequent solution system. At the same time, the urea group in the thiourea structure it contains can also interact with the copper surface, so that the amino compound is easy to form a passivation film on the copper surface, has good film-forming stability, reduces the contact between the copper surface and the corrosive medium, and thus achieves the effect of inhibiting metal corrosion. In addition, the amino compound can coordinate with the copper ions on the chip surface and the solution system, exists in the form of a stable soluble complex, and is taken away from the chip surface with the flowing cleaning solution to achieve a good cleaning effect.

[0037] In particular, chitosan oligosaccharide aminothiourea Schiff base has an amino and urea-modified Schiff base structure and a thiourea structure, and has the properties of an inhibitor and a cleaning liquid. It can be adsorbed on the copper surface to form a passivation film to replace the oxide layer, inhibit the contact between the corrosive medium and the copper surface, and prevent further oxidation of copper, thereby playing an excellent corrosion inhibition role on the chip. Its hydrophilicity and water solubility give it excellent solubility, ensuring the stability of the entire solution system. Its coordination with copper ions can accelerate the dissolution of the copper surface oxide layer, and has a strong chelating effect on the copper metal ions in the solution, reacting with copper ions to form a stable and soluble complex to achieve the effect of cleaning the residue on the surface of the semiconductor chip.

[0038] 2) The amino compound and the chelating agent of the present invention are used simultaneously to chelate copper ions and inhibit copper corrosion, accelerate the dissolution of the copper surface oxide layer, and can form a stable complex with more copper ions, thereby improving the cleaning effect of the entire system. At the same time, the molecular structure of the chelating agent has a strong adsorption capacity of P heteroatom and a hydrophilic group, which further enhances the adsorption of the amino compound on the metal surface, and is easy to form a coordination bond with the copper surface, replacing the oxide layer on the copper surface to prevent further oxidation of copper, and having a better corrosion inhibition effect on the chip, thereby promoting the adsorption of the cleaning solution on the copper surface to slow down corrosion, and ensuring that the surface of the semiconductor chip is smooth and low in corrosion after cleaning.

[0039] 3) The pH regulator of the present invention can provide a suitable acidic environment to dissolve the oxide layer and other residual pollutants on the copper surface, chelate the copper ions in the solution, enhance the cleaning effect, and form a hydrophobic film on the copper surface with long-chain alkyl groups as hydrophobic branches, further enhancing the corrosion inhibition effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a microscope picture of the Cu wafer before cleaning, magnified 100 times;

[0041] Figure 2 This is a microscope picture magnified 100 times after the Cu wafer is cleaned with the cleaning solution of Example 1;

[0042] Figure 3 This is a microscope picture magnified 100 times after the Cu wafer was cleaned with the cleaning solution of Comparative Example 3. DETAILED DESCRIPTION

[0043] The present invention is further described below with reference to the examples. The description of the technical features described below is based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that:

[0044] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0045] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B.

[0046] In the present specification, a numerical range expressed using "above" or "below" means a numerical range including the number.

[0047] In this specification, the word "may" means both performing a certain process and not performing a certain process.

[0048] In this specification, the use of "optional" or "optional" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used.

[0049] In this specification, when "normal temperature" or "room temperature" is used, the temperature may be 15-25°C.

[0050] In this manual, the reagents or instruments used without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.

[0051] Examples 1-6

[0052] Examples 1-6 disclose a variety of low metal corrosion chip post-CMP cleaning solutions, the components and weight ratios of which are shown in Table 1. The preparation method is as follows: weigh each component in its respective amount, mix and dissolve all the components completely to obtain the low metal corrosion chip post-CMP cleaning solution.

[0053] Table 1 Components and weight ratios of low metal corrosion chip post-CMP cleaning solution

[0054]

[0055]

[0056] Comparative Examples 1-4

[0057] Comparative Examples 1-4 disclose a variety of cleaning solutions, the components and weight ratios of which are shown in Table 2, and the preparation methods thereof are the same as those of Example 1.

[0058] Table 2 Components and weight ratios of the cleaning solution

[0059]

[0060]

[0061] The various properties of the above embodiments or comparative examples are tested below.

[0062] The corrosion rate test results are shown in Table 3. It can be seen that after the chip is cleaned with the cleaning solution prepared in Examples 1-6 of the present invention, there is almost no corrosion mark, and the corrosion rate is The corrosion rate of comparative examples 1-4 is greater than That is to say, there is a certain amount of corrosion in Comparative Examples 1-4 compared with Examples 1-6. Specifically, Comparative Example 1 uses a conventional triazole amino compound, and Comparative Example 2 uses a conventional aminophosphonic acid chelating agent. Although they have a good cleaning effect, their corrosion rate is significantly increased compared with Example 1, and both have a certain amount of corrosion on copper. Comparative Example 3 does not add an amino compound, and the corrosion rate increases, proving that the corrosion inhibition effect is relatively poor. Comparative Example 4 uses inorganic acid phosphoric acid as a pH regulator. Although it can ensure that the system is acidic, it cannot achieve chelation of copper ions, and the corrosion inhibition effect is poor.

[0063] Table 3 Test results of Examples 1-6 and Comparative Examples 1-4

[0064]

[0065] in:

[0066] The test method for metal corrosion is static corrosion test:

[0067] Step 1: Cut the copper wafer into 2cm*2cm square pieces, and pre-treat with 3wt% citric acid solution at room temperature for 5min, wash with ultrapure water, and blow dry with nitrogen;

[0068] Step 2: Use a microscope to take a picture of the copper wafer, see Figure 1 The copper wafer film thickness and resistivity were tested with four probes to determine the functional relationship between copper thickness and resistivity, which was used to calculate the copper corrosion rate ( Right now );

[0069] Step 3: Take another 30 mL of cleaning solution and soak the copper wafer for 10 hours at room temperature for static corrosion, then rinse with ultrapure water and blow dry with nitrogen;

[0070] Step 4: Use a microscope to take pictures of the copper wafer after corrosion for comparison, see Figure 2 and Figure 3 The film thickness of the copper wafer after corrosion was tested with four probes, and then the corrosion rate was calculated according to the change in the thickness of the copper wafer before and after corrosion, so as to investigate the corrosion of the metal by different cleaning solutions. The test results are shown in Table 3.

[0071] Figure 1 This is a microscope picture of the Cu wafer before cleaning, magnified 100 times; Figure 2 This is a microscope picture magnified 100 times after the Cu wafer is cleaned with the cleaning solution of Example 1; Figure 3 This is a microscope picture magnified 100 times after the Cu wafer was cleaned with the cleaning solution of Comparative Example 3. It can be seen that the Cu wafer cleaned with the cleaning solution of Example 1 is almost not corroded, while the Cu wafer cleaned with the cleaning solution of Comparative Example 3 has a rough surface and is severely corroded.

[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A low metal corrosion chip CMP cleaning solution, characterized in that: The composition includes the following components in weight ratio:

2. The low metal corrosion chip post-CMP cleaning solution according to claim 1, characterized in that: The amino compound is an amino organic urea.

3. The low metal corrosion chip post-CMP cleaning solution according to claim 1, characterized in that: The chelating agent is an organic phosphine derivative.

4. The low metal corrosion chip post-CMP cleaning solution according to claim 1, characterized in that: The pH regulator is one or more of DL-malic acid, itaconic acid, gluconic acid, agaric acid and quinic acid.

5. The low metal corrosion chip post-CMP cleaning solution according to claim 1, characterized in that: The low metal corrosion chip post-CMP cleaning solution is acidic.

6. The low metal corrosion chip post-CMP cleaning solution according to claim 1 or 5, characterized in that: The pH value of the post-CMP cleaning solution for chips with low metal corrosion is 2-6.

7. A method for preparing a post-CMP cleaning solution for a chip with low metal corrosion according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: weighing each component respectively, mixing and dissolving all the components completely, and obtaining the chip post-CMP cleaning solution with low metal corrosion.

8. Use of the chip post-CMP cleaning solution with low metal corrosion as claimed in any one of claims 1 to 6 in the field of cleaning semiconductor chips.

9. The use according to claim 8, characterized in that: The method for cleaning a semiconductor chip using the chip post-CMP cleaning solution with low metal corrosion comprises the following steps: Step 1: preparing the low metal corrosion chip post-CMP cleaning solution with ultrapure water into an aqueous solution with a mass concentration of 10-100%, and then using the aqueous solution to soak a semiconductor chip at room temperature to obtain a soaked semiconductor chip; Step 2: Rinse the soaked semiconductor chip in ultrapure water to complete the cleaning process of the semiconductor chip.

10. The use according to claim 9, characterized in that: The soaking time in step 1 is 5-30 minutes.