Method for recovering copper from precious lead
Through the combination of vacuum distillation, hydrogen peroxide oxidation and electrodisposition, the problems of high energy consumption and low recovery in traditional precious lead are solved, and the process flow is streamlined and efficient copper recycling is achieved, with copper recovery rate reaching 85-90 %.
Patent Information
- Application Number
- CN202411142810.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
The traditional copper recycling method in precious lead has problems such as high energy consumption and low copper recovery rate, and the process flow is complex and not streamlined enough.
Using a combination of vacuum distillation, hydrogen peroxide oxidative leaching and electrodistribution, volatiles and residues are obtained by vacuum distillation, acidic leaching is performed using hydrogen peroxide and sulfuric acid, and subsequent electrodistribution is performed to obtain high-purity cathode copper.
The process flow is shortened and the copper recovery is efficient. The copper recovery rate reaches 85-90%, and energy consumption is significantly reduced.
Smart Images

Figure CN119020604A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of metallurgical engineering technology, and in particular to a method for recovering copper from precious lead. Background Art
[0002] Precious lead is the main intermediate product of the precious metal silver metallurgical process. It is rich in gold, silver, copper, lead, bismuth and antimony and has high value. Production companies have conducted research on the recovery of valuable metals in precious lead. Traditionally, there are two main methods for the recovery of copper in precious lead:
[0003] (1) Precious lead is put into a reverberatory furnace (or converter) and smelted at 900-950℃ to remove antimony and produce a high-copper precious alloy. The high-copper precious alloy is then put into a copper removal pot and smelted at 380-410℃ to remove copper. It is then refined at 700-750℃ to remove tellurium and produce copper-free and tellurium-containing precious lead. The precious lead is distilled in a vacuum furnace to produce a high-silver residue, which is then smelted in a silver separation furnace to remove impurities and produce crude silver. The crude silver is electrolyzed to obtain high-purity silver. Crude copper is obtained by blowing and oxidizing the matte slag produced by smelting and removing copper to remove lead, antimony and bismuth.
[0004] (2) Precious lead is put into a reverberatory furnace (or converter) for smelting at 900-950°C to remove antimony and produce a high-copper and high-silver alloy. The high-copper and high-silver alloy is directly transferred to a silver separation furnace for smelting to remove lead, bismuth and copper to produce crude silver. The crude silver is electrolyzed to obtain silver products. At the same time, a large amount of converter slag is produced and returned to the blast furnace for reduction smelting to produce alloys and molten copper matte. The molten copper matte is then smelted and oxidized to remove lead, antimony and bismuth to obtain crude copper.
[0005] Both of the above methods can achieve copper recovery. However, the problem is that the crude copper recovered in method (1) is obtained by blowing and oxidizing the matte slag produced by smelting and removing copper to remove lead, antimony and bismuth. The recovery rate and purity of copper depend on the smelting and copper removal and oxidative blowing processes. Since the above recovery processes are all pyrometallurgical processes, they have high temperature requirements and lead to high energy consumption. The recovery of copper in method (2) is also completely a pyrometallurgical process, and the energy consumption is also high. Furthermore, both of the above methods have the problem of low direct copper recovery rate.
[0006] How to achieve efficient copper recovery while shortening the process has always been a technical problem that needs to be solved urgently by technicians in this field. Summary of the invention
[0007] In order to solve or partially solve the problems existing in the related art, the present application provides a method for recovering copper from precious lead, which achieves efficient recovery of copper on the basis of shortening the process flow.
[0008] A method for recovering copper from precious lead in the present application is carried out according to the following steps:
[0009] (1) subjecting the precious lead to vacuum distillation to obtain volatile matter and residue;
[0010] (2) adding sulfuric acid to the obtained residue under the condition of hydrogen peroxide as an oxidant for acid leaching, and filtering to obtain a copper sulfate leachate;
[0011] (3) The copper sulfate leaching solution is subjected to electrolysis to obtain cathode copper.
[0012] Furthermore, the vacuum degree of the vacuum distillation is 5-30 Pa, the distillation temperature is 600-700° C., and the distillation time is 5-10 h.
[0013] Furthermore, the acid leaching temperature is 70-80°C, the leaching time is 10-20 hours, and 7-8 mL of sulfuric acid is added per gram of residue during leaching; the amount of hydrogen peroxide added is 10-20 mL per m 3 Add 50-150 l of sulfuric acid; pH value at leaching end point: 1.0-2.0.
[0014] Furthermore, the electrodeposition temperature is 30-50°C, and the current density is 150-180A / m 2 .
[0015] Furthermore, the precious lead contains 2-3% copper, 13-18% lead, 18-24% antimony, 6-10% bismuth, 10-20% silver, 5-8% arsenic, and 200-300 g / t gold.
[0016] Furthermore, the cathode copper contains ≥99.9% copper, <0.0005% bismuth, <0.005% lead, <0.025% silver, and the total impurities are <0.03%.
[0017] The beneficial effects of this application are:
[0018] When the precious lead is processed to recover copper, the present application only needs to recover copper through vacuum distillation, hydrogen peroxide oxidation leaching and electrowinning. Compared with the traditional method of recovering copper from precious lead, the present application has fewer steps and a more streamlined process. The method in the present application achieves efficient recovery of copper on the basis of shortening the process flow, and the direct recovery rate of copper is 85-90%. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram of the process flow in this application. DETAILED DESCRIPTION
[0020] The embodiments of the present application will be described in more detail below with reference to examples. Although the embodiments of the present application are shown in the examples, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present application more thorough and complete, and the scope of the present application can be fully communicated to those skilled in the art.
[0021] Example 1
[0022] A method for recovering copper from precious lead in this embodiment is carried out according to the following steps:
[0023] (1) subjecting precious lead to vacuum distillation to obtain volatiles and residues; wherein the chemical composition of the precious lead is as follows: 2-3% copper, 13-18% lead, 18-24% antimony, 6-10% bismuth, 10-20% silver, 5-8% arsenic, and 200-300 g / t gold;
[0024] The vacuum degree of vacuum distillation is 5-30Pa, the distillation temperature is 600-700℃, and the distillation time is 5-10h;
[0025] (2) adding sulfuric acid to the obtained residue under the condition of hydrogen peroxide as an oxidant for acid leaching, and filtering to obtain a copper sulfate leachate;
[0026] Specifically, the acid leaching temperature is 70-80°C, the leaching time is 10-20 hours, and 7 mL of sulfuric acid is added per gram of residue during leaching; the amount of hydrogen peroxide added is 3 100L of sulfuric acid was added; pH value at the leaching end point was 1.5;
[0027] (1) electrolytically depositing the copper sulfate leaching solution to obtain cathode copper; wherein the electrolytic deposition control conditions are a temperature of 30 to 50° C. and a current density of 150 to 180 A / m 2 .
[0028] Among them, in this embodiment, the direct recovery rate of copper from precious lead to electrode copper is 85%.
[0029] Example 2
[0030] A method for recovering copper from precious lead in this embodiment is carried out according to the following steps:
[0031] (1) subjecting precious lead to vacuum distillation to obtain volatiles and residues; wherein the chemical composition of the precious lead is as follows: 2-3% copper, 13-18% lead, 18-24% antimony, 6-10% bismuth, 10-20% silver, 5-8% arsenic, and 200-300 g / t gold;
[0032] The vacuum degree of vacuum distillation is 5-30Pa, the distillation temperature is 600-700℃, and the distillation time is 5-10h;
[0033] (2) adding sulfuric acid to the obtained residue under the condition of hydrogen peroxide as an oxidant for acid leaching, and filtering to obtain a copper sulfate leachate;
[0034] Specifically, the acid leaching control conditions are: temperature of 70-80°C, leaching time of 10-20h, adding 8mL sulfuric acid per gram of residue during leaching; the amount of hydrogen peroxide added is 1mL per gram of residue. 3 150L of sulfuric acid was added; pH value at the leaching end point was 2.0;
[0035] (3) electrolytically depositing the copper sulfate leaching solution to obtain cathode copper; wherein the electrolytic deposition control conditions are a temperature of 30 to 50° C. and a current density of 150 to 180 A / m 2 .
[0036] Among them, in this embodiment, the direct recovery rate of copper from precious lead to electrode copper is 87.5%.
[0037] Example 3
[0038] A method for recovering copper from precious lead in this embodiment is carried out according to the following steps:
[0039] (1) subjecting precious lead to vacuum distillation to obtain volatiles and residues; wherein the chemical composition of the precious lead is as follows: 2-3% copper, 13-18% lead, 18-24% antimony, 6-10% bismuth, 10-20% silver, 5-8% arsenic, and 200-300 g / t gold;
[0040] The vacuum degree of vacuum distillation is 5-30Pa, the distillation temperature is 600-700℃, and the distillation time is 5-10h;
[0041] (2) adding sulfuric acid to the obtained residue under the condition of hydrogen peroxide as an oxidant for acid leaching, and filtering to obtain a leachate;
[0042] Specifically, the acid leaching control conditions are: temperature of 70-80°C, leaching time of 10-20h, adding 7.5mL sulfuric acid per gram of residue during leaching; the amount of hydrogen peroxide added is 3 Sulfuric acid was added 50L; pH value at leaching end point was 1.0;
[0043] (3) electrolytically depositing the leaching solution to obtain cathode copper; wherein the electrolytic deposition control conditions are a temperature of 30 to 50° C. and a current density of 150 to 180 A / m 2 .
[0044] Among them, in this embodiment, the direct recovery rate of copper from precious lead to electrode copper is 90%.
[0045] The embodiments of the present application have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
Claims
1. A method for recovering copper from precious lead, characterized in that: Follow these steps: (1) subjecting the precious lead to vacuum distillation to obtain volatile matter and residue; (2) adding sulfuric acid to the obtained residue under the condition of hydrogen peroxide as an oxidant for acid leaching, and filtering to obtain a copper sulfate leachate; (3) The copper sulfate leaching solution is subjected to electrolysis to obtain cathode copper.
2. A method for recovering copper from precious lead according to claim 1, characterized in that: The vacuum degree of the vacuum distillation is 5-30 Pa, the distillation temperature is 600-700° C., and the distillation time is 5-10 hours.
3. A method for recovering copper from precious lead according to claim 1, characterized in that: The acid leaching temperature is 70-80°C, the leaching time is 10-20h, and 7-8mL sulfuric acid is added per gram of residue during leaching; the amount of hydrogen peroxide added is 3 Add 50-150L of sulfuric acid; pH value at leaching endpoint: 1.0-2.
0.
4. A method for recovering copper from precious lead according to claim 1, characterized in that: The electroplating temperature is 30-50°C and the current density is 150-180A / m 2 .
5. A method for recovering copper from precious lead according to claim 1, characterized in that: The precious lead contains 2-3% copper, 13-18% lead, 18-24% antimony, 6-10% bismuth, 10-20% silver, 5-8% arsenic and 200-300g / t gold.
6. A method for recovering copper from precious lead according to claim 1, characterized in that: The cathode copper contains ≥99.9% copper, <0.0005% bismuth, <0.005% lead, <0.025% silver, and the total impurities are <0.03%.