Recycling and regenerating process of waste rare earth polishing powder

The waste rare earth polishing powder is processed by sodium hydroxide, complexing agent, dispersing agent and fluorinating agent, and the impurities are removed at high temperature and calcination are removed, which solves the problems of high recycling costs and large waste liquid generation, and achieves efficient regeneration rare earth polishing The production of powder is suitable for polishing and processing of precision optical glass.

CN119020619APending Publication Date: 2024-11-26XIAN RARE METAL MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411151613.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the recycling cost of rare earth polishing powder is high and a large amount of alkali-containing waste liquid and waste residue is generated, resulting in high waste of rare earth resources and treatment costs.

Method used

Sodium hydroxide, complexing agent, dispersant and fluorinating agent are used to treat waste rare earth polishing powder, remove Al2O3 and SiO2 impurities under high temperature reflux conditions, and remove organic impurities by roasting to obtain efficient regenerated rare earth polishing powder, and recycle alkali to reduce waste liquid production.

Benefits of technology

It achieves efficient removal of impurities, reduces recycling costs, improves the polishing effect and crystallinity of regenerated rare earth polishing powder, simplifies the process flow, and is suitable for polishing and processing of precision optical glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020619A_ABST
    Figure CN119020619A_ABST
Patent Text Reader

Abstract

The invention discloses a waste rare earth polishing powder recycling and regenerating process which comprises the following steps: step 1, crushing waste rare earth polishing powder through wet ball milling, dispersing in an ethylene glycol-water system, adding sodium hydroxide, a complexing agent, a dispersing agent and a fluorinating agent, mixing, and shearing and dispersing to obtain slurry to be treated; 2, reacting the to-be-treated slurry, heating and refluxing, and centrifuging to obtain alkali liquor and solid particles; and thirdly, the solid particles are washed, dried and roasted, and the regenerated rare earth polishing powder is obtained. According to the regeneration technology, sodium hydroxide, a complexing agent, a dispersing agent and a fluorinating agent are adopted for treating the waste rare earth polishing powder, main impurities such as Al2O3 and SiO2 can be efficiently removed under the high-temperature backflow condition, zeolite substances are prevented from being formed, other organic matter impurities are removed through roasting treatment, and the regenerated rare earth polishing powder with the good polishing effect is obtained; the invention is applicable to the technical field of polishing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polishing, and in particular relates to a recycling process of waste rare earth polishing powder. Background Art

[0002] Chemical mechanical polishing (CMP) is an industrial technology for ultra-precision machining. It is widely used in precision optics, aerospace, information technology and other fields because it can perfectly balance global flatness, material surface defects and reliability. From a global perspective, CMP rare earth polishing materials still have a relatively broad market.

[0003] In recent years, with the rapid development of precision optics and precision semiconductor processing industries, China's consumption of rare earth polishing powder has increased by 10% each year. At the same time, tens of thousands of tons of rare earth polishing powder waste are generated every year. Unfortunately, the current waste rare earth polishing powder is still mainly treated by traditional methods such as shelving or landfilling, resulting in a large waste of rare earth resources. As a major country in the mining and application of rare earth resources, my country has developed a waste rare earth polishing powder recycling process, which can not only save the mining of primary rare earth mineral resources and reduce the waste of rare earth resources, but also generate certain economic value, which is of great significance to my country's rare earth industry.

[0004] For example, the Chinese invention patent "A method for preparing rare earth oxide from waste rare earth polishing powder" (Announcement No. CN103103361B) treats waste rare earth polishing powder with alkali roasting, and then obtains rare earth oxide products through water washing, acid leaching, washing, oxalic acid precipitation and high-temperature calcination, so that the acid-insoluble structures such as LaF3, LaOF or CeO2 in the waste rare earth polishing powder react under the action of molten salt and are converted into acid-soluble rare earth oxide or rare earth hydroxide; however, this method has high recovery costs and produces a large amount of alkaline waste liquid and waste residue. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies in the above-mentioned prior art and provide a recycling and regeneration process for waste rare earth polishing powder. The recycling process uses sodium hydroxide, a complexing agent, a dispersant and a fluorinating agent to treat the waste rare earth polishing powder, and can efficiently remove major impurities such as Al2O3 and SiO2 under high-temperature reflux conditions and avoid the formation of zeolite substances. The remaining organic impurities are removed by roasting to obtain regenerated rare earth polishing powder with good polishing effect. At the same time, the alkali solution separated in the regeneration process can be recycled, which solves the problem of large amount of alkali-containing waste liquid and waste residue generated after recycling the waste rare earth polishing powder in the prior art.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a recycling and regeneration process of waste rare earth polishing powder, characterized in that the process comprises the following steps:

[0007] Step 1: crushing the waste rare earth polishing powder by wet ball milling, dispersing it in an ethylene glycol-water system, adding sodium hydroxide, a complexing agent, a dispersant and a fluorinating agent to mix, and then shearing and dispersing it to obtain a slurry to be treated;

[0008] Step 2: subjecting the slurry to be treated obtained in step 1 to an impurity removal reaction at 60° C. to 85° C., heating to 120° C. to 140° C. for reflux treatment, and then centrifuging to obtain an alkali solution and solid particles;

[0009] Step 3: Wash, dry and calcine the solid particles obtained in step 2 to obtain regenerated rare earth polishing powder.

[0010] The present invention adopts an ethylene glycol-water system to disperse the waste rare earth polishing powder, has good dispersing effect and can reduce the probability of secondary agglomeration of the waste rare earth polishing powder, helps the waste rare earth polishing powder to fully contact with sodium hydroxide, a complexing agent and a fluorinating agent, and cooperates with the dispersant to improve the impurity removal efficiency; and by adding a fluorinating agent to supplement the fluorine content of the waste rare earth polishing powder, the polishing force of the waste rare earth polishing powder is restored.

[0011] The present invention controls the impurity removal reaction temperature in step 2 to 60°C to 85°C, which is conducive to the dissolution of sodium hydroxide and fluoriding agent and enables them to be in uniform contact with the waste rare earth polishing powder particles, and allows the complexing agent to be combined with Al in the slurry to be treated. 3+ 、Na + Complexation reaction occurs, thereby reducing the insoluble Na (x / q) [(AlO2) x (SiO2) y ]·n(H2O) zeolite precipitation is produced to reduce the polishing scratch rate of the recycled polishing powder; by raising the temperature to 120℃~140℃ for reflux, the silicon and aluminum substances in the waste rare earth polishing powder can be fully dissolved, thereby achieving the purpose of removing impurities in the waste rare earth polishing powder.

[0012] The above-mentioned recycling and regeneration process of waste rare earth polishing powder is characterized in that the ball-to-material ratio used in the wet ball milling in step one is 5:1, the wet ball milling uses ethanol as the medium, and the mass ratio of the ethanol to the waste rare earth polishing powder is 5:1.

[0013] The above-mentioned recycling and regeneration process of waste rare earth polishing powder is characterized in that in the ethylene glycol-water system in step one, the volume ratio of ethylene glycol to water is 1:2 to 1:4.

[0014] The invention is used to achieve a good dispersion effect of waste rare earth polishing powder by controlling the volume ratio of ethylene glycol to water.

[0015] The above-mentioned recycling and regeneration process of waste rare earth polishing powder is characterized in that the mass of sodium hydroxide in step one accounts for 26% to 40% of the total mass of the slurry to be treated, the mass of the dispersant accounts for 1.3% to 2% of the total mass of the slurry to be treated, the concentration of the complexing agent in the slurry to be treated is 0.05moL / L to 0.1moL / L, the mass of the fluorinating agent is 1.5% to 2% of the mass of the waste rare earth polishing powder, and the fluorinating agent is KF.

[0016] The above-mentioned recycling and regeneration process of waste rare earth polishing powder is characterized in that the complexing agent in step one is one of ethylenediaminetetraacetic acid, urea and acetylacetone, and the dispersant is one of polyvinyl pyrrolidone, hydroxypropyl cellulose and polyethylene glycol.

[0017] The above-mentioned recycling and regeneration process of waste rare earth polishing powder is characterized in that the shearing and dispersion in step one adopts a shearing machine, and the shearing machine speed is 10000rpm~12000rpm.

[0018] The invention can improve the dispersion degree of polishing powder particles in the slurry to be processed and reduce particle agglomeration by adopting high-speed shear dispersion.

[0019] The above-mentioned recycling and regeneration process of waste rare earth polishing powder is characterized in that the reflux treatment time in step 2 is 2h to 4h, and the centrifugal speed is 6000rpm to 8000rpm.

[0020] The above-mentioned recycling and regeneration process of waste rare earth polishing powder is characterized in that the alkali solution in step 2 is added to the slurry to be treated obtained in step 1 for recycling, and sodium hydroxide is added to the alkali solution before recycling so that the pH of the alkali solution is 13-14, and the alkali solution can be recycled 4-6 times.

[0021] The above-mentioned recycling and regeneration process of waste rare earth polishing powder is characterized in that the washing in step three adopts deionized water and industrial ethanol, the drying temperature is 60°C to 90°C, and the roasting temperature is 800°C to 1000°C.

[0022] The present invention can quickly dry the solid particles after centrifugation by controlling the drying temperature to 60°C-90°C; and can remove organic impurities in the polishing powder by controlling the roasting temperature to 800°C-1000°C, thereby improving the density of the regenerated rare earth polishing powder and the crystallinity of the regenerated rare earth polishing powder, thereby improving the polishing ability.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] 1. The present invention uses sodium hydroxide, a complexing agent, a dispersant and a fluorinating agent to treat waste rare earth polishing powder. Under high-temperature reflux conditions, it can effectively remove major impurities such as Al2O3 and SiO2, avoid the formation of hard and insoluble zeolite substances, and remove the remaining organic impurities through roasting treatment to obtain regenerated rare earth polishing powder with good polishing effect; the alkaline solution obtained by centrifugal separation during the regeneration process can be used for the recycling treatment of the next batch of waste rare earth polishing powder, which is beneficial to reducing the treatment cost of the waste rare earth polishing powder.

[0025] 2. The present invention adopts an ethylene glycol-water system in combination with a dispersant and performs a high-speed shear dispersion treatment, which can effectively improve the dispersibility of the slurry, inhibit the agglomeration and agglomeration of the waste rare earth polishing powder, and thus improve the impurity removal effect.

[0026] 3. The present invention supplements the fluorine content of the waste rare earth polishing powder by adding a fluorinating agent, and performs high-temperature calcination to improve the crystallinity of the regenerated rare earth polishing powder, thereby improving the polishing ability of the regenerated rare earth polishing powder.

[0027] 4. The process of the present invention is short, the operation is simple, and it is easy to scale up for industrial production. The recovery rate of the prepared rare earth polishing powder exceeds 90%, and the final product can be directly used for fine polishing of optical glass.

[0028] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 1 is the XRD diagram of the regenerated rare earth polishing powder prepared in Example 1 and the waste rare earth polishing powder before regeneration.

[0030] Figure 2 This is an atomic force microscope image of H-K9 optical glass polished with the regenerated rare earth polishing powder prepared in Example 1.

[0031] Figure 3 This is a graph showing the roughness results of H-K9 optical glass polished with the regenerated rare earth polishing powder prepared in Example 1. DETAILED DESCRIPTION

[0032] Example 1

[0033] The process of this embodiment includes the following steps:

[0034] Step 1, 50g of waste rare earth polishing powder is put into a ball mill with 250g of ethanol as a ball milling medium for wet ball milling, and then the crushed waste rare earth polishing powder is dispersed in an ethylene glycol-water system, and 161.53g of sodium hydroxide, 8.27g of polyvinyl pyrrolidone, 8.67g of ethylenediaminetetraacetic acid and 1g of KF are added to mix, and shear dispersion is performed at a speed of 10000rpm for 1h to obtain a slurry to be treated; the waste rare earth polishing powder is a mixed waste rare earth polishing powder provided by Northern Optoelectronics Group, the ethylene glycol-water system is a mixed solution of 100mL of ethylene glycol and 200mL of deionized water, and the ball mill uses 250g of steel balls as grinding balls;

[0035] Step 2: Stir the slurry to be treated obtained in step 1 at 80° C. for 2 h, then heat to 120° C. for reflux treatment for 4 h, and centrifuge the slurry after natural cooling to obtain alkali solution and solid particles; the centrifugal speed is 8000 rpm;

[0036] Step 3: Wash the solid particles obtained in step 2 with deionized water for 3 times, dry them in an oven at 60° C. for 5 h, and then calcine them in a muffle furnace at 1000° C. to obtain regenerated rare earth polishing powder.

[0037] XRD analysis was performed on the regenerated rare earth polishing powder prepared in this embodiment and the waste rare earth polishing powder before regeneration. Figure 1 As shown in the figure, the main phases of waste rare earth polishing powder are CeO2, La2O3, CeLa2O3F3 and LaOF. Since SiO2 is glass and Al2O3 comes from the flocculant used in the polishing process, both are amorphous and do not have obvious characteristic peaks in the XRD spectrum. Therefore, Si and Al elements are not shown in the XRD spectrum of waste rare earth polishing powder; the main phases of recycled rare earth polishing powder have not changed significantly, but the crystallinity is significantly improved compared with that of waste rare earth polishing powder.

[0038] The regenerated rare earth polishing powder of this embodiment is used to polish H-K9 optical glass, and the surface roughness of the polished H-K9 optical glass is tested using an atomic force microscope. Figure 2 and Figure 3 As shown, after polishing with recycled rare earth polishing powder, the surface of H-K9 glass has high flatness, no obvious scratches and low roughness.

[0039] The components of the regenerated rare earth polishing powder prepared in Example 1 and the waste rare earth polishing powder that was not regenerated in step 1 were analyzed, as shown in Table 1.

[0040] Table 1 Composition of recycled rare earth polishing powder and waste rare earth polishing powder

[0041] Element <![CDATA[CeO2]]> <![CDATA[La2O3]]> <![CDATA[Pr6O 11 ]]> <![CDATA[Nd2O3]]> other Comparative Example 1 Waste rare earth polishing powder 57.6% 30.1% 3.6% 4.9% 3.8% Example 1 Regenerated rare earth polishing powder 60.1% 30.6% 3.2% 4.5% 1.6%

[0042] It can be seen from Table 1 that the mass proportion of other impurities in waste rare earth polishing powder is twice that of recycled rare earth polishing powder, indicating that the effective polishing components in waste rare earth polishing powder are less than those in recycled rare earth polishing powder. After regeneration, the impurities in the recycled rare earth polishing powder can be effectively removed.

[0043] Example 2

[0044] The process of this embodiment includes the following steps:

[0045] Step 1, put 100g of waste rare earth polishing powder into a ball mill with 500g of ethanol as the ball milling medium for wet ball milling, then disperse the crushed waste rare earth polishing powder in an ethylene glycol-water system and add 400g of sodium hydroxide, 15.0g of polyvinyl pyrrolidone, 17.34g of ethylenediaminetetraacetic acid and 2g of KF to mix, and shear disperse for 1h at a speed of 12000rpm to obtain a slurry to be treated; the waste rare earth polishing powder is a mixed waste rare earth polishing powder provided by Northern Optoelectronics Group, the ethylene glycol-water system is a mixed solution of 200mL of ethylene glycol and 400mL of deionized water, and the ball mill uses 500g of steel balls as grinding balls;

[0046] Step 2: react the slurry to be treated obtained in step 1 at 85° C. for 2 h, then heat to 140° C. for reflux treatment for 2 h, and centrifuge the slurry after natural cooling to obtain alkali solution and solid particles; the centrifugal speed is 6000 rpm;

[0047] Step 3: Wash the solid particles obtained in step 2 with deionized water for 3 times, dry them in an oven at 60° C. for 5 h, and then calcine them in a muffle furnace at 800° C. to obtain regenerated rare earth polishing powder.

[0048] Example 3

[0049] The process of this embodiment includes the following steps:

[0050] Step 1, put 25g of waste rare earth polishing powder into a ball mill with 125g of ethanol as a ball milling medium for wet ball milling, then disperse the crushed waste rare earth polishing powder in an ethylene glycol-water system and add 128g of sodium hydroxide, 8.56g of polyethylene glycol, 17.34g of ethylenediaminetetraacetic acid and 0.5g of KF to mix, and shear disperse for 1h at a speed of 11000rpm to obtain a slurry to be treated; the waste rare earth polishing powder is a mixed waste rare earth polishing powder provided by Northern Optoelectronics Group, the ethylene glycol-water system is a mixed solution of 100mL of ethylene glycol and 200mL of deionized water, and the ball mill uses 125g of steel balls as grinding balls;

[0051] Step 2: react the slurry to be treated obtained in step 1 at 70° C. for 2 h, then heat to 120° C. for reflux treatment for 4 h, and centrifuge the slurry after natural cooling to obtain alkali solution and solid particles; the centrifugal speed is 8000 rpm;

[0052] Step 3: Wash the solid particles obtained in step 2 with deionized water for 3 times, dry them in an oven at 60° C. for 5 h, and then calcine them in a muffle furnace at 1000° C. to obtain regenerated rare earth polishing powder.

[0053] Example 4

[0054] The process of this embodiment includes the following steps:

[0055] Step 1, put 150g of waste rare earth polishing powder into a ball mill with 750g of ethanol as the ball milling medium for wet ball milling, then disperse the crushed waste rare earth polishing powder in an ethylene glycol-water system and add 600g of sodium hydroxide, 30g of hydroxypropyl cellulose, 9.0g of acetylacetone and 3g of KF to mix, and shear and disperse for 1h at a speed of 10000rpm to obtain a slurry to be treated; the waste rare earth polishing powder is a mixed waste rare earth polishing powder provided by Northern Optoelectronics Group, the ethylene glycol-water system is a mixed solution of 300mL of ethylene glycol and 600mL of deionized water, and the ball mill uses 750g of steel balls as grinding balls;

[0056] Step 2: react the slurry to be treated obtained in step 1 at 60° C. for 2 h, then heat to 120° C. for reflux treatment for 3 h, and centrifuge the slurry after reflux treatment after natural cooling to obtain alkali solution and solid particles; the centrifugal speed is 8000 rpm;

[0057] Step 3: Wash the solid particles obtained in step 2 with deionized water for 3 times, dry them in an oven at 90° C. for 5 h, and then calcine them in a muffle furnace at 1000° C. to obtain regenerated rare earth polishing powder.

[0058] Example 5

[0059] The process of this embodiment includes the following steps:

[0060] Step 1, put 200g of waste rare earth polishing powder into a ball mill with 1000g of ethanol as the ball milling medium for wet ball milling, then disperse the crushed waste rare earth polishing powder in an ethylene glycol-water system and add 800g of sodium hydroxide, 40g of polyethylene glycol, 7.20g of urea and 4g of KF to mix, and shear and disperse for 1h at a speed of 10000rpm to obtain a slurry to be treated; the waste rare earth polishing powder is a mixed waste rare earth polishing powder provided by Northern Optoelectronics Group, the ethylene glycol-water system is a mixed solution of 400mL of ethylene glycol and 800mL of deionized water, and the ball mill uses 1000g of steel balls as grinding balls;

[0061] Step 2: react the slurry to be treated obtained in step 1 at 80° C. for 2 h, then heat to 120° C. for reflux treatment for 2 h, and centrifuge the slurry after reflux treatment after natural cooling to obtain alkali solution and solid particles; the centrifugal speed is 8000 rpm;

[0062] Step 3: Wash the solid particles obtained in step 2 with industrial ethanol for three times, dry them in an oven at 90° C. for 5 h, and then calcine them in a muffle furnace at 800° C. to obtain regenerated rare earth polishing powder.

[0063] Example 6

[0064] The difference between this embodiment and embodiment 5 is that: in step 1, 200g of waste rare earth polishing powder is put into a ball mill with 1000g of ethanol as a ball milling medium for wet ball milling, and then the crushed waste rare earth polishing powder is dispersed in an ethylene glycol-water system and 800g of sodium hydroxide, 62g of polyethylene glycol, 50g of urea, 3g of KF and 50mL of alkali solution obtained in step 2 of embodiment 5 are added and mixed; the ethylene glycol-water system is a mixed solution of 300mL of ethylene glycol and 1200mL of deionized water, and the alkali solution is centrifuged and sodium hydroxide is added to make the pH of the alkali solution 13.8.

[0065] Example 7

[0066] The difference between this embodiment and embodiment 5 is that: in step 1, 200g of waste rare earth polishing powder is put into a ball mill with 1000g of ethanol as the ball milling medium for wet ball milling, and then the crushed waste rare earth polishing powder is dispersed in an ethylene glycol-water system and 800g of sodium hydroxide, 40g of polyethylene glycol, 5.9g of urea and 3.3g of KF are added to mix; the ethylene glycol-water system is a mixed solution of 400mL of ethylene glycol and 1000mL of deionized water.

[0067] The polishing performance test was carried out on the regenerated rare earth polishing powder obtained in Examples 1 to 7, the mixed waste rare earth polishing powder provided by Northern Optoelectronics Group, and the 1650 waste rare earth polishing powder. The polishing test was carried out using Shenyang Kejing UNIPOL-1200S single-sided polishing machine and a polyurethane polishing pad. The polishing sample was a circular optical H-K9 glass substrate with a diameter of 3 cm. The glass substrate was pre-roughly polished and the surface roughness (Ra) was 10 nm. The feed rate of the rare earth polishing liquid was 40 mL / min, the mass proportion of the polishing abrasive in the polishing slurry was 1%, the polishing pressure was 3.5 kg, the polishing time was 10 min, the upper polishing disc speed was 80 rpm, and the lower polishing disc speed was 80 rpm.

[0068] After polishing, the polished glass substrate is scrubbed, spun dry, ultrasonically cleaned with pure water, and dried. The polishing rate of the glass substrate is then determined by measuring the change in mass before and after polishing, and the surface roughness of the glass substrate is measured by an atomic force microscope.

[0069] Table 2 Polishing performance

[0070] Cutting rate (nm / min) Surface roughness(nm) Example 1 780 0.32 Example 2 720 0.51 Example 3 680 0.72 Example 4 770 0.66 Example 5 620 0.74 Example 6 700 0.70 Example 7 710 0.69 Mixed waste rare earth polishing powder 287.6 1.21 1650 type waste rare earth polishing powder 365.1 0.88

[0071] It can be seen from Table 2 that the polishing rate of the regenerated rare earth polishing powder of Examples 1 to 7 is not less than 620 nm / min, and the surface roughness is not greater than 0.74; under the condition that the mass proportion of polishing abrasive is 1%, the polishing rate of the mixed waste rare earth polishing powder and 1650 type waste rare earth polishing powder that have not been treated by the regeneration process is significantly reduced and the surface roughness is significantly increased compared with Examples 1 to 7, indicating that the polishing performance of the waste rare earth polishing powder that has not been treated by the regeneration process is poor, and the regeneration process of the present invention can effectively improve the polishing performance of the regenerated rare earth polishing powder.

[0072] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A process for recycling waste rare earth polishing powder, characterized in that: The process includes the following steps: Step 1: crushing the waste rare earth polishing powder by wet ball milling, dispersing it in an ethylene glycol-water system, adding sodium hydroxide, a complexing agent, a dispersant and a fluorinating agent to mix, and then shearing and dispersing it to obtain a slurry to be treated; Step 2: subjecting the slurry to be treated obtained in step 1 to an impurity removal reaction at 60° C. to 85° C., heating to 120° C. to 140° C. for reflux treatment, and then centrifuging to obtain an alkali solution and solid particles; Step 3: Wash, dry and calcine the solid particles obtained in step 2 to obtain regenerated rare earth polishing powder.

2. The recycling process of waste rare earth polishing powder according to claim 1, characterized in that: The ball-to-material ratio used in the wet ball milling in step one is 5:1, the wet ball milling uses ethanol as the medium, and the mass ratio of the ethanol to the waste rare earth polishing powder is 5:

1.

3. The recycling process of waste rare earth polishing powder according to claim 1, characterized in that: The volume ratio of ethylene glycol to water in the ethylene glycol-water system in step 1 is 1:2 to 1:

4.

4. The recycling process of waste rare earth polishing powder according to claim 1, characterized in that: In step one, the mass of sodium hydroxide accounts for 26% to 40% of the total mass of the slurry to be treated, the mass of the dispersant accounts for 1.3% to 2% of the total mass of the slurry to be treated, the concentration of the complexing agent in the slurry to be treated is 0.05moL / L to 0.1moL / L, the mass of the fluorinating agent is 1.5% to 2% of the mass of the waste rare earth polishing powder, and the fluorinating agent is KF.

5. The recycling process of waste rare earth polishing powder according to claim 1, characterized in that: In step 1, the complexing agent is one of ethylenediaminetetraacetic acid, urea and acetylacetone, and the dispersant is one of polyvinyl pyrrolidone, hydroxypropyl cellulose and polyethylene glycol.

6. The recycling process of waste rare earth polishing powder according to claim 1, characterized in that: The shearing and dispersion in step 1 adopts a shearing machine, and the speed of the shearing machine is 10000rpm~12000rpm.

7. The recycling process of waste rare earth polishing powder according to claim 1, characterized in that: The reflux treatment time in step 2 is 2h to 4h, and the centrifugal speed is 6000rpm to 8000rpm.

8. The process for recycling waste rare earth polishing powder according to claim 1, characterized in that: The alkali solution in step 2 is added to the slurry to be treated obtained in step 1 for recycling. Before the alkali solution is recycled, sodium hydroxide is added to make the pH of the alkali solution 13-14. The alkali solution can be recycled 4-6 times.

9. The recycling process of waste rare earth polishing powder according to claim 1, characterized in that: In step 3, the washing is carried out using deionized water or industrial ethanol, the drying temperature is 60°C to 90°C, and the calcination temperature is 800°C to 1000°C.