Manufacturing method of low-yield-ratio pipeline steel for longitudinal welded pipe

By employing specific smelting and hot rolling processes, pipeline steel with a low yield strength ratio for straight seam welded pipes is produced, solving the problems of high cost and insufficient performance, and realizing the production of low-cost, high-performance pipeline steel.

CN119020662APending Publication Date: 2024-11-26BAOTOU IRON & STEEL (GROUP) CO LTD

Patent Information

Application Number
CN202411058211.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing technologies for producing high-strength pipeline steel suffer from high costs and difficulty in achieving excellent overall performance and service performance while ensuring a low yield strength ratio.

Method used

By employing specific smelting and hot rolling processes, including molten iron pretreatment, LF refining, RH refining, and casting machine production, and in conjunction with specific chemical compositions and hot rolling parameters, such as billet heating temperature, mill type, and cooling method, pipeline steel for straight seam welded pipes with low yield strength ratio is prepared.

Benefits of technology

The produced pipeline steel plates have a yield strength ratio of <0.86, excellent tensile and impact properties, low alloy cost, and are suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020662A_ABST
    Figure CN119020662A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of low-yield-ratio pipeline steel for a longitudinal welded pipe. The manufacturing method comprises the following steps: smelting and continuous casting production process flow: molten iron pretreatment, converter treatment, LF (ladle furnace) refining, RH (Ruhrstahl Heraeus) refining and machine casting; the molten steel for a casting machine comprises the following chemical components in percentage by mass: 0.13 to 0.15 percent of C, 0.10 to 0.20 percent of Si, 1.05 to 1.20 percent of Mn, less than or equal to 0.010 percent of P, less than or equal to 0.005 percent of S, 0.010 to 0.020 percent of Nb, 0.010 to 0.020 percent of Ti and the balance of Fe and other inevitable impurities. The hot rolling production process comprises the steps of casting blank heating, rough rolling, finish rolling and coiling. The produced pipeline steel plate has excellent tensile property and impact property, the yield ratio is smaller than 0.86, and meanwhile, the alloy is low in cost, simple in preparation method and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgical plate production, and in particular relates to a method for manufacturing low-yield ratio pipeline steel for straight seam welded pipes. Background Art

[0002] Pipeline transportation is the most economical and reasonable way to transport oil and natural gas over long distances. With the increase in demand for oil and natural gas, pipeline steel has developed rapidly. In order to improve transportation efficiency, reduce energy consumption and reduce investment, long-distance pipelines are developing in the direction of high pressure and large diameter transportation. At the same time, pipeline steel is required to have high strength, high toughness and high purity. At present, the higher the grade of pipeline steel, the lower its carbon content and the higher the amount of alloy elements added. This means that while the quality grade of pipeline steel continues to improve, its production cost also increases accordingly.

[0003] In recent years, the technology and quality of the steel industry have developed rapidly, and the demand for high-quality pipeline steel has further increased at home and abroad. In addition, due to the influence of the market environment, major companies have strict requirements for cost control of steel. Therefore, how to ensure the low cost of steel strip while obtaining excellent comprehensive performance and service performance is of great research significance for enhancing the market competitiveness of pipeline steel. Summary of the invention

[0004] The purpose of the present invention is to provide a method for manufacturing low-yield ratio pipeline steel for straight seam welded pipes. The pipeline steel plate produced by the present invention has excellent tensile properties and impact properties, and the yield ratio is less than 0.86. At the same time, the alloy cost of the present invention is low, the preparation method is simple, and it is suitable for industrial production.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] The present invention discloses a method for manufacturing low yield ratio pipeline steel for straight seam welded pipe, comprising:

[0007] (1) Smelting-continuous casting production process: molten iron pretreatment-converter-LF refining-RH refining-casting machine; the chemical composition of the molten steel supplied to the casting machine is C: 0.13-0.15%, Si: 0.10-0.20%, Mn: 1.05-1.20%, P≤0.010%, S≤0.005%, Nb: 0.010-0.020%, Ti 0.010-0.020%, and the balance is Fe and other unavoidable impurities;

[0008] (2) Hot rolling production process: heating of ingot - rough rolling - finishing rolling - coiling; the ingot is smelted and cast into slab, heated to 1190-1220℃, and hot-charged in the furnace for 160-270min; the soaking temperature is 1170-1210℃, and the soaking time is 20-45min; the rough rolling adopts a 2-stand rolling mill, and the rough rolling temperature is 970-990℃; the finishing rolling adopts a 7-stand continuous variable crown rolling mill, and the finishing rolling temperature is 835-865℃, and the thickness of the hot rolled steel strip is 7.1mm; the cooling adopts laminar cooling equipment, and the coiling temperature is 635-665℃.

[0009] Furthermore, the chemical composition of the pipeline steel in terms of mass percentage is C: 0.14%, Si: 0.18%, Mn: 1.10%, P: 0.008%, S: 0.003%, Nb: 0.015%, Ti 0.013%, and the remainder is Fe and other inevitable impurities.

[0010] Furthermore, the chemical composition of the pipeline steel in terms of mass percentage is C: 0.14%, Si: 0.14%, Mn: 1.13%, P: 0.008%, S: 0.003%, Nb: 0.013%, Ti 0.016%, and the remainder is Fe and other inevitable impurities.

[0011] Furthermore, the chemical composition of the pipeline steel in mass percentage is C: 0.15%, Si: 0.16%, Mn: 1.15%, P: 0.009%, S: 0.004%, Nb: 0.015%, Ti 0.015%, and the remainder is Fe and other inevitable impurities.

[0012] Furthermore, the heating temperature is 1205°C, the hot charging time in the furnace is 230min; the soaking temperature is 1192°C, and the hot charging soaking time is 35min;

[0013] The starting temperature of rough rolling is 1185°C, and the cumulative reduction of rough rolling is 84%;

[0014] The cumulative reduction of finishing rolling is 85%, ensuring the final rolling temperature of finishing rolling is 853℃;

[0015] The coiling temperature is 608°C;

[0016] The finished product thickness is 7.1mm.

[0017] Furthermore, the heating temperature is 1208°C, the hot charging time in the furnace is 235min; the soaking temperature is 1193°C, and the hot charging soaking time is 32min;

[0018] The starting temperature of rough rolling is 1183°C, and the cumulative reduction of rough rolling is 84%;

[0019] The cumulative reduction of finishing rolling is 84%, ensuring the final rolling temperature of finishing rolling is 850℃;

[0020] The coiling temperature is 603°C;

[0021] The finished product thickness is 7.1mm.

[0022] Furthermore, the heating temperature is 1206°C, the hot charging time in the furnace is 232 min; the soaking temperature is 1192°C, and the hot charging soaking time is 34 min;

[0023] The starting temperature of rough rolling is 1185°C, and the cumulative reduction of rough rolling is 84%;

[0024] The cumulative reduction of finishing rolling is 85%, ensuring the final rolling temperature of finishing rolling is 852℃;

[0025] The coiling temperature is 606°C;

[0026] The finished product thickness is 7.1mm.

[0027] Furthermore, the yield strength ratio of the produced pipeline steel plate is less than 0.86.

[0028] Furthermore, the mechanical properties of the produced pipeline steel are stable and meet the standard requirements.

[0029] Compared with the prior art, the beneficial technical effects of the present invention are:

[0030] The granular bainite grains of the pipeline steel plate produced by the present invention are fine and evenly distributed. The pipeline steel plate produced by the method provided by the present invention has a yield strength ratio of less than 0.86, and various properties are stable and meet the standard requirements. At the same time, the alloy of the present invention has low cost, simple preparation method, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The present invention will be further described below in conjunction with the accompanying drawings.

[0032] Figure 1 This is the microstructure diagram of the steel plate at 1 / 2 of Example 1 of the present invention;

[0033] Figure 2 This is the microstructure diagram of the steel plate at 1 / 4 of Example 1 of the present invention. DETAILED DESCRIPTION

[0034] The present invention is described in more detail below through specific examples. The examples are merely descriptions of the best mode of implementation of the present invention and do not limit the scope of the present invention in any way.

[0035] Example 1

[0036] The chemical composition of the casting machine in the embodiment of the present invention is shown in Table 1.

[0037] In the embodiment of the present invention, the heating temperature is 1205° C., the hot charging time in the furnace is 230 min, the soaking temperature is 1192° C., and the hot charging soaking time is 35 min.

[0038] The starting rolling temperature in the embodiment of the present invention is 1185° C., and the cumulative reduction of the rough rolling is 84%.

[0039] In the embodiment of the present invention, the cumulative reduction of the finishing rolling is 85%, and the final rolling temperature of the finishing rolling is ensured to be 853°C.

[0040] The coiling temperature in the embodiment of the present invention is 608°C.

[0041] The thickness of the finished product in the embodiment of the present invention is 7.1 mm.

[0042] Example 2

[0043] The chemical composition of the casting machine in the embodiment of the present invention is shown in Table 1.

[0044] In the embodiment of the present invention, the heating temperature is 1208° C., the hot charging time in the furnace is 235 min, the soaking temperature is 1193° C., and the hot charging soaking time is 32 min.

[0045] The starting rolling temperature in the embodiment of the present invention is 1183° C., and the cumulative reduction of the rough rolling is 84%.

[0046] In the embodiment of the present invention, the cumulative reduction of the finishing rolling is 84%, and the final rolling temperature of the finishing rolling is ensured to be 850°C.

[0047] The coiling temperature in the embodiment of the present invention is 603°C.

[0048] The thickness of the finished product in the embodiment of the present invention is 7.1 mm.

[0049] Example 3

[0050] The chemical composition of the casting machine in the embodiment of the present invention is shown in Table 1.

[0051] In the embodiment of the present invention, the heating temperature is 1206° C., the hot charging time in the furnace is 232 min, the soaking temperature is 1192° C., and the hot charging soaking time is 34 min.

[0052] The starting rolling temperature in the embodiment of the present invention is 1185° C., and the cumulative reduction of the rough rolling is 84%.

[0053] In the embodiment of the present invention, the cumulative reduction of the finishing rolling is 85%, and the final rolling temperature of the finishing rolling is ensured to be 852°C.

[0054] The coiling temperature in the embodiment of the present invention is 606°C.

[0055] The thickness of the finished product in the embodiment of the present invention is 7.1 mm.

[0056] Table 1 Chemical composition of Examples 1 to 3 of the present invention (wt%)

[0057] Example C Si Mn P S Nb Ti O 1 0.14 0.18 1.10 0.008 0.003 0.015 0.013 0.0015 2 0.14 0.14 1.13 0.008 0.003 0.013 0.016 0.0023 3 0.15 0.16 1.15 0.009 0.004 0.015 0.015 0.0017

[0058] The steel coils of Examples 1 to 3 of the present invention were tested for mechanical properties, and the test results are shown in Table 2.

[0059] Table 2 Mechanical properties of the steel coils of Examples 1 to 3 of the present invention

[0060]

[0061] It can be seen from Table 2 that the mechanical properties and process properties of the pipeline steel for straight seam welded pipe produced according to the method provided by the present invention meet the standard requirements.

[0062] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for manufacturing low yield ratio pipeline steel for straight seam welded pipe, characterized in that: include: (1) Smelting-continuous casting production process: molten iron pretreatment-converter-LF refining-RH refining-casting machine; the chemical composition of the molten steel supplied to the casting machine is C: 0.13-0.15%, Si: 0.10-0.20%, Mn: 1.05-1.20%, P≤0.010%, S≤0.005%, Nb: 0.010-0.020%, Ti 0.010-0.020%, and the balance is Fe and other unavoidable impurities; (2) Hot rolling production process: heating of ingot - rough rolling - finishing rolling - coiling; the ingot is smelted and cast into slab, heated to 1190-1220℃, and hot-charged in the furnace for 160-270min; the soaking temperature is 1170-1210℃, and the soaking time is 20-45min; the rough rolling adopts a 2-stand rolling mill, and the rough rolling temperature is 970-990℃; the finishing rolling adopts a 7-stand continuous variable crown rolling mill, and the finishing rolling temperature is 835-865℃, and the thickness of the hot rolled steel strip is 7.1mm; the cooling adopts laminar cooling equipment, and the coiling temperature is 635-665℃.

2. The method for manufacturing low yield ratio pipeline steel for straight seam welded pipe according to claim 1, characterized in that: The chemical composition of the pipeline steel in mass percentage is C: 0.14%, Si: 0.18%, Mn: 1.10%, P: 0.008%, S: 0.003%, Nb: 0.015%, Ti 0.013%, and the remainder is Fe and other inevitable impurities.

3. The method for manufacturing low yield ratio pipeline steel for straight seam welded pipe according to claim 1, characterized in that: The chemical composition of the pipeline steel in mass percentage is C: 0.14%, Si: 0.14%, Mn: 1.13%, P: 0.008%, S: 0.003%, Nb: 0.013%, Ti 0.016%, and the remainder is Fe and other inevitable impurities.

4. The method for manufacturing low yield ratio pipeline steel for straight seam welded pipe according to claim 1, characterized in that: The chemical composition of the pipeline steel in mass percentage is C: 0.15%, Si: 0.16%, Mn: 1.15%, P: 0.009%, S: 0.004%, Nb: 0.015%, Ti 0.015%, and the remainder is Fe and other inevitable impurities.

5. The method for manufacturing low yield ratio pipeline steel for straight seam welded pipe according to claim 2, characterized in that: The heating temperature is 1205℃, and the hot charging time in the furnace is 230min; the soaking temperature is 1192℃, and the hot charging soaking time is 35min; The starting temperature of rough rolling is 1185°C, and the cumulative reduction of rough rolling is 84%; The cumulative reduction of finishing rolling is 85%, ensuring the final rolling temperature of finishing rolling is 853℃; The coiling temperature is 608°C; The finished product thickness is 7.1mm.

6. The method for manufacturing low yield ratio pipeline steel for straight seam welded pipe according to claim 3, characterized in that: The heating temperature is 1208℃, and the hot charging time in the furnace is 235min; the soaking temperature is 1193℃, and the hot charging soaking time is 32min; The starting temperature of rough rolling is 1183°C, and the cumulative reduction of rough rolling is 84%; The cumulative reduction of finishing rolling is 84%, ensuring the final rolling temperature of finishing rolling is 850℃; The coiling temperature is 603°C; The finished product thickness is 7.1mm.

7. The method for manufacturing low yield ratio pipeline steel for straight seam welded pipe according to claim 4, characterized in that: The heating temperature is 1206℃, and the hot charging time in the furnace is 232min; the soaking temperature is 1192℃, and the hot charging soaking time is 34min; The starting temperature of rough rolling is 1185°C, and the cumulative reduction of rough rolling is 84%; The cumulative reduction of finishing rolling is 85%, ensuring the final rolling temperature of finishing rolling is 852℃; The coiling temperature is 606°C; The finished product thickness is 7.1mm.

8. The method for manufacturing low yield ratio pipeline steel for straight seam welded pipe according to claim 1, characterized in that: The yield strength ratio of the produced pipeline steel plate is less than 0.

86.

9. The method for manufacturing low yield ratio pipeline steel for straight seam welded pipe according to claim 8, characterized in that: The mechanical properties of the produced pipeline steel are stable and meet the standard requirements.

Citation Information

Patent Citations

  • X80 pipeline steel used for longitudinal resistance welded pipe and method for producing its hot rolled coil

    CN102400054A

  • Quenched and tempered low-yield ratio pipeline steel and preparation method thereof

    CN104674114A

  • X65 pipeline steel and production method thereof

    CN105063483A

  • X52MS hot rolled coil plate for high-frequency resistance weld pipe and manufacturing method thereof

    CN107988547A

  • Bridge structural steel Q345qE steel strip with low-temperature toughness and production method thereof

    CN109023064A

Cited By

  • Thin-gauge low-yield-ratio L245-L450 pipeline steel as well as preparation method and application thereof

    CN122279421A