Method for directly alloying low-grade titanium slag
By mixing low-grade titanium slag with iron concentrate and lime, using aluminum powder and potassium chlorate as reducing agents, conducting aluminum-thermal self-propagation reaction, and directly alloying to obtain titanium ferroalloy, solving the problem of unutilized titanium resources and realizing titanium resources efficient short process utilization and environmental development.
Patent Information
- Application Number
- CN202411064575.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The titanium content in traditional vanadium titanium ore is relatively low, resulting in the failure of efficient utilization of titanium resources, long process flow and high production costs, resulting in loss of titanium resources and environmental pollution.
Low-grade titanium slag, iron concentrate and lime are mixed in a certain proportion, aluminum powder and potassium chlorate are added as reducing agents, and directly alloyed through aluminum-heat self-propagation reaction to obtain titanium ferro-alloy, simplifying the process flow and reducing environmental pressure.
It realizes the efficient utilization of short processes of low-grade titanium slag, reduces production costs, promotes the green development of titanium resources, avoids traditional strong acid reduction processes, and reduces environmental pressure.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of efficient utilization of titanium slag, and particularly relates to a method for direct alloying of low-grade titanium slag. Background Art
[0002] At present, the titanium content in traditional vanadium-titanium ore is relatively low. If titanium resources are to be extracted and utilized efficiently, the vanadium-titanium ore needs to be reduced to obtain titanium slag. Titanium slag cannot be directly used to extract titanium due to its low grade, so it is necessary to enrich the titanium-containing slag to obtain high-titanium slag. The high-titanium slag is reduced by sulfuric acid or chlorination to finally obtain titanium products such as titanium dioxide or sponge titanium. From vanadium-titanium ore to the final titanium product, the process is long, and the subsequent reduction process involves a large number of chemical processes and acid-containing materials. Not only is the process control difficult, but the production cost is also high, making it difficult to promote industrialization.
[0003] In view of the above reasons, in the current process of utilizing vanadium-titanium ore resources, only iron and vanadium resources are extracted and utilized, and a large amount of titanium resources remain in the slag. A large amount of titanium-containing slag is still treated in the form of stockpiling and has not been utilized in a high-value manner. This not only causes the loss of titanium resources, but also the stockpiling of a large amount of solid waste, seriously affecting the ecological environment. Summary of the invention
[0004] The purpose of the present invention is to provide a method for direct alloying of low-grade titanium slag, which realizes the short-process and efficient utilization of low-grade titanium slag while reducing environmental pressure and promoting the green development of the titanium resource industry.
[0005] To achieve the above purpose, the technical solution provided by the present invention is as follows: A method for direct alloying of low-grade titanium slag, specifically comprising: mixing low-grade titanium slag, iron concentrate and slag-forming agent lime in a certain proportion and drying them, mixing them with a reducing agent, and then adding them into a smelting furnace, initiating an aluminothermic reduction reaction by ignition, and standing and cooling after the reaction is completed, separating the slag from the gold, and obtaining a titanium-iron alloy.
[0006] Furthermore, the low-grade titanium slag of the present invention is a titanium-containing byproduct produced during the reduction and smelting of vanadium-titanium ore. 2 The content is 45%~55%.
[0007] Furthermore, the low-grade titanium slag of the present invention has a MgO content of ≤4.5%, a CaO content of ≤5.5%, and a SiO 2 Content ≤20%, FeO content ≤5%.
[0008] Furthermore, the Fe 2 O 3 content ≥90%, MgO content ≤4.5%, CaO content ≤5.5%, SiO 2Content ≤8.5%, Al 2 O 3 Content ≤1%, S content ≤0.06%, P content ≤0.02%, Mn content ≤0.06%.
[0009] Furthermore, the mixing ratio of the low-grade titanium slag and the iron ore concentrate in the present invention is m:m in the range of 1:1 to 2:1.
[0010] Furthermore, the mixing ratio m:m of the low-grade titanium slag and the slag-forming agent lime of the present invention is 2:1 to 4:1.
[0011] Furthermore, the drying of the present invention is carried out by heating in a rotary kiln, and the materials can be mixed again during the heating process; the drying temperature is controlled at 300-600°C, preferably 450-600°C, and the drying time is 2-5 hours, preferably 3.5-5 hours, to ensure the dehydration and mixing effect of the materials.
[0012] Furthermore, the reducing agent of the present invention is a mixture of aluminum powder and potassium chlorate, wherein the addition amount of the aluminum powder is 20% to 35% of the total material, and the addition amount of the potassium chlorate is 10% to 20% of the total material.
[0013] Preferably, the particle size of the aluminum powder of the present invention is ≤2 mm.
[0014] Furthermore, the smelting furnace of the present invention is made of cast iron, and the bottom of the furnace body is covered with magnesia sand, which can help separate the smelted material from the furnace body.
[0015] Furthermore, the materials after adding the reducing agent described in the present invention are added to the smelting furnace in batches, specifically: a portion of the materials after adding the reducing agent is first added to the smelting furnace, and then the remaining materials are added in batches after ignition to allow all the materials to react fully.
[0016] Furthermore, the composition of the titanium-iron alloy of the present invention is Ti: 25-35%, Al: 7.0-8.0%, Si: 1.0-3.0%, C: 0.04-0.1%, Mn: 0.9-1.35%, Cu: 0.02-0.05%, S: 0.02-0.03%, P: 0.01-0.02%, Fe: balance, which conforms to the titanium-iron alloy standard GB / T3282-2012.
[0017] The inventive principle and beneficial technical effects of the present invention are: The present invention uses low-grade titanium slag obtained by reducing and melting vanadium-titanium ore as raw material, and mixes it with a certain proportion of iron concentrate as iron-containing raw material, and uses aluminum powder and potassium chlorate as reducing agents, and lime as slag-making agent. After the materials are fully mixed, the titanium in the titanium slag and the iron in the iron concentrate are directly reduced by aluminothermic self-propagating reaction, and the metal titanium and metal iron obtained after reduction directly form titanium-iron alloy at high temperature. In order to ensure the full progress of the reaction, a mixture of aluminum powder and potassium chlorate is innovatively selected as an efficient reducing agent. This method can directly alloy low-grade titanium slag to obtain titanium-iron alloy. While realizing the short-process efficient utilization of low-grade titanium slag, it avoids the traditional strong acid reduction to extract titanium, greatly reduces environmental pressure, and promotes the green development of the titanium resource industry.
[0018] The present invention uses aluminum powder and potassium chlorate as reducing agents, which can ensure that titanium oxide and iron oxide are fully reduced during the aluminothermic self-propagating reaction. Aluminum powder is more likely to undergo redox reaction than aluminum particles and aluminum blocks, and adding potassium chlorate can further increase the reaction rate, especially in the process of spontaneously exothermic aluminothermic reaction, adding potassium chlorate can promote the reaction.
[0019] The present invention uses iron concentrate as the iron-containing raw material, which ensures that the reaction heat is fully released and can also reduce production costs, thereby achieving industrial large-scale application and promotion. DETAILED DESCRIPTION
[0020] The present technology is further described below in conjunction with more specific embodiments. Example 1
[0021] A method for direct alloying of low-grade titanium slag comprises the following steps: The low-grade titanium slag obtained after the reduction and smelting of vanadium-titanium ore, iron concentrate and slag-making agent lime were mixed in a mass ratio of 2:2:1, and then added into a rotary kiln for heating and drying. The drying temperature was controlled at 500°C and the drying time was 3.5 hours. 2 The content is 48%, the MgO content is 4.0%, the CaO content is 5.0%, and the SiO 2 The content is 15%, and the FeO content is 3.5%; the Fe content in the iron concentrate used is 2 O 3 The content is 91%, MgO content is 4.0%, CaO content is 5.0%, SiO 2 The content is 8.0%, Al 2 O 3 The content is 0.5%, the S content is 0.03%, the P content is 0.01%, and the Mn content is 0.04%.
[0022] (2) Mix the dried material with the reducing agent aluminum powder (particle size ≤ 2mm) and potassium chlorate, wherein the amount of aluminum powder added is 20% of the total material, and the amount of potassium chlorate added is 15% of the total material. After the material mixed with the reducing agent is fully mixed, add it into the smelting furnace body made of cast iron. First, add 20% of the total amount, use magnesium rod to ignite, and initiate the aluminum thermal reduction reaction. During the reaction, add the remaining material into the furnace body in 4 batches.
[0023] (3) After the material is fully reacted, it is naturally cooled for 48 hours, and then the slag and gold are separated to obtain titanium-iron alloy.
[0024] The titanium-iron alloy prepared in this embodiment was analyzed for composition, and the results were: Ti: 28.35%, Al: 7.9%, Si: 1.26%, C: 0.04%, Mn: 1.21%, Cu: 0.02%, S: 0.03%, P: 0.008%, Fe: balance, which meets the standard GB / T3282-2012. Example 2
[0025] A method for direct alloying of low-grade titanium slag comprises the following steps: The low-grade titanium slag obtained after the reduction and smelting of vanadium-titanium ore, iron concentrate and slag-making agent lime were mixed in a mass ratio of 7.5:5:3, and then added into a rotary kiln for heating and drying. The drying temperature was controlled at 550°C and the drying time was 4 hours. 2 The content is 50%, MgO content is 4.1%, CaO content is 4.8%, SiO 2 The content is 18.5%, and the FeO content is 3.0%; the Fe content in the iron concentrate used is 2 O 3 The content is 92%, MgO content is 3.5%, CaO content is 4.0%, SiO 2 The content is 6.0%, Al 2 O 3 The content is 0.4%, the S content is 0.04%, the P content is 0.02%, and the Mn content is 0.03%.
[0026] (2) Mix the dried material with the reducing agent aluminum powder (particle size ≤ 2mm) and potassium chlorate, wherein the amount of aluminum powder added is 20% of the total material, and the amount of potassium chlorate added is 10% of the total material. After the material mixed with the reducing agent is fully mixed, add it into the smelting furnace body made of cast iron. First, add 20% of the total amount, use magnesium rod to ignite, and initiate the aluminum thermal reduction reaction. During the reaction, add the remaining material into the furnace body in 4 times.
[0027] (3) After the material is fully reacted, it is naturally cooled for 48 hours, and then the slag and gold are separated to obtain titanium-iron alloy.
[0028] The titanium-iron alloy prepared in this embodiment was analyzed for composition, and the results were: Ti: 32.35%, Al: 7.51%, Si: 2.65%, C: 0.06%, Mn: 1.28%, Cu: 0.03%, S: 0.03%, P: 0.01%, Fe: balance, which meets the standard GB / T3282-2012. Example 3
[0029] A method for direct alloying of low-grade titanium slag comprises the following steps: The low-grade titanium slag obtained after the reduction and smelting of vanadium-titanium ore, iron concentrate and slag-making agent lime are mixed in a mass ratio of 2:1:1, and then added into a rotary kiln for heating and drying. The drying temperature is controlled at 600°C and the drying time is 4 hours. 2 The content is 55%, the MgO content is 3.2%, the CaO content is 4.6%, and the SiO 2 The content is 19.5%, and the FeO content is 3.0%; the Fe content in the iron concentrate used is 2 O 3 The content is 93%, MgO content is 3.5%, CaO content is 4.0%, SiO 2 The content is 6.5%, Al 2 O 3 The content of Al is 0.5%, the content of S is 0.05%, the content of P is 0.01%, and the content of Mn is 0.04%.
[0030] (2) Mix the dried material with the reducing agent aluminum powder (particle size ≤ 2mm) and potassium chlorate, wherein the amount of aluminum powder added is 30% of the total material, and the amount of potassium chlorate added is 15% of the total material. After fully mixing the material mixed with the reducing agent, add it into the cast iron smelting furnace body, first add 20% of the total amount, use magnesium rod to ignite, and initiate the aluminum thermal reduction reaction. During the reaction, add the remaining material into the furnace body in 4 times.
[0031] (3) After the material is fully reacted, it is naturally cooled for 48 hours, and then the slag and gold are separated to obtain titanium-iron alloy.
[0032] The titanium-iron alloy prepared in this embodiment was subjected to composition analysis, and the results were: Ti: 34.07%, Al: 7.65%, Si: 1.48%, C: 0.05%, Mn: 1.26%, Cu: 0.04%, S: 0.016%, P: 0.009%, Fe: balance, which meets the titanium-iron alloy GB / T3282-2012 standard. Example 4
[0033] A method for direct alloying of low-grade titanium slag comprises the following steps: The low-grade titanium slag obtained after the reduction and smelting of vanadium-titanium ore, iron concentrate and slag-making agent lime were mixed in a mass ratio of 6:3:2, and then added into a rotary kiln for heating and drying. The drying temperature was controlled at 550°C and the drying time was 5 hours. 2 The content is 52.5%, MgO content is 2.9%, CaO content is 4.1%, SiO 2 The content is 16.5%, and the FeO content is 3.5%; the Fe content in the iron concentrate used is 2 O 3 The content is 95%, the MgO content is 2.5%, the CaO content is 2.5%, and the SiO 2 The content is 7.2%, Al 2 O 3 The content is 0.6%, the S content is 0.03%, the P content is 0.01%, and the Mn content is 0.03%.
[0034] (2) Mix the dried material with the reducing agent aluminum powder (particle size ≤ 2mm) and potassium chlorate, wherein the amount of aluminum powder added is 25% of the total material, and the amount of potassium chlorate added is 20% of the total material. After the material mixed with the reducing agent is fully mixed, add it into the smelting furnace body made of cast iron. First, add 20% of the total amount, ignite it with magnesium rods, and initiate the aluminum thermal reduction reaction. During the reaction, add the remaining material into the furnace body in 4 times.
[0035] (3) After the material is fully reacted, it is naturally cooled for 48 hours, and then the slag and gold are separated to obtain titanium-iron alloy.
[0036] The titanium-iron alloy prepared in this embodiment was analyzed for composition, and the results were: Ti: 33.45%, Al: 7.13%, Si: 1.67%, C: 0.06%, Mn: 1.19%, Cu: 0.02%, S: 0.026%, P: 0.009%, Fe: balance, which meets the standard GB / T3282-2012. Example 5
[0037] A method for direct alloying of low-grade titanium slag comprises the following steps: The low-grade titanium slag obtained after the reduction and smelting of vanadium-titanium ore, iron concentrate and slag-making agent lime are mixed in a mass ratio of 4:2:1, and then added into a rotary kiln for heating and drying. The drying temperature is controlled at 450°C and the drying time is 5 hours. 2 The content is 51.8%, the MgO content is 2.5%, the CaO content is 3.5%, and the SiO 2 The content is 17.2%, and the FeO content is 3.0%; the Fe content in the iron concentrate used is 2 O 3The content is 93%, MgO content is 2.5%, CaO content is 5.0%, SiO 2 The content is 5.5%, Al 2 O 3 The content is 0.8%, the S content is 0.03%, the P content is 0.01%, and the Mn content is 0.03%.
[0038] (2) Mix the dried material with the reducing agent aluminum powder (particle size ≤ 2mm) and potassium chlorate, wherein the amount of aluminum powder added is 35% of the total material, and the amount of potassium chlorate added is 20% of the total material. After the material mixed with the reducing agent is fully mixed, add it into the smelting furnace body made of cast iron. First, add 20% of the total amount, use magnesium rod to ignite, and initiate the aluminum thermal reduction reaction. During the reaction, add the remaining material into the furnace body in 4 times.
[0039] (3) After the material is fully reacted, it is naturally cooled for 48 hours, and then the slag and gold are separated to obtain titanium-iron alloy.
[0040] The titanium-iron alloy prepared in this embodiment was analyzed for composition, and the results were: Ti: 32.34%, Al: 7.1%, Si: 1.12%, C: 0.05%, Mn: 1.14%, Cu: 0.03%, S: 0.03%, P: 0.01%, Fe: balance, which meets the standard GB / T3282-2012.
Claims
1. A method for direct alloying of low-grade titanium slag, characterized in that: Specifically, low-grade titanium slag, iron ore concentrate and slag-forming agent lime are mixed and dried in a certain proportion, mixed with a reducing agent, and then added into a smelting furnace. An aluminothermic reduction reaction is initiated by ignition. After the reaction is completed, the reaction is allowed to stand and cool, and the slag and gold are separated to obtain titanium-iron alloy.
2. The method for direct alloying of low-grade titanium slag according to claim 1, characterized in that: The TiO2 content in the low-grade titanium slag is 45% to 55%.
3. The method for direct alloying of low-grade titanium slag according to claim 1, characterized in that: The low-grade titanium slag has a MgO content of ≤4.5%, a CaO content of ≤5.5%, a SiO2 content of ≤20%, and a FeO content of ≤5%.
4. The method for direct alloying of low-grade titanium slag according to claim 1, characterized in that: The iron concentrate has a Fe2O3 content of ≥90%, a MgO content of ≤4.5%, a CaO content of ≤5.5%, a SiO2 content of ≤8.5%, an Al2O3 content of ≤1%, a S content of ≤0.06%, a P content of ≤0.02%, and a Mn content of ≤0.06%.
5. The method for direct alloying of low-grade titanium slag according to claim 1, characterized in that: The mixing ratio of the low-grade titanium slag and the iron ore concentrate is m:m in the range of 1:1 to 2:1; the mixing ratio of the low-grade titanium slag and the slag-forming agent lime is m:m in the range of 2:1 to 4:
1.
6. The method for direct alloying of low-grade titanium slag according to claim 1, characterized in that: The drying temperature is 300-600° C., and the drying time is 2-5 hours.
7. The method for direct alloying of low-grade titanium slag according to claim 1, characterized in that: The reducing agent is a mixture of aluminum powder and potassium chlorate, wherein the addition amount of the aluminum powder is 20% to 35% of the total material, and the addition amount of the potassium chlorate is 10% to 20% of the total material.
8. The method for direct alloying of low-grade titanium slag according to claim 7, characterized in that: The particle size of the aluminum powder is ≤2 mm.
9. The method for direct alloying of low-grade titanium slag according to claim 1, characterized in that: The titanium-iron alloy composition complies with the standard GB / T3282-2012.
10. The method for direct alloying of low-grade titanium slag according to claim 1, characterized in that: The titanium-iron alloy comprises Ti: 25-35%, Al: 7.0-8.0%, Si: 1.0-3.0%, C: 0.04-0.1%, Mn: 0.9-1.35%, Cu: 0.02-0.05%, S: 0.02-0.03%, P: 0.01-0.02%, and Fe: balance.
Citation Information
Patent Citations
Calcium-magnesium-titanium method for producing high ferrotitanium alloy
CN104152694A
Titanium-iron alloy preparation method
CN106834891A
CHARGE FOR PRODUCING TITANIUM-CONTAINING SLAG, TITANIUM-CONTAINING CHARGE AND A METHOD FOR ALUMINOTHERMAL PRODUCTION OF FERROTITANIUM USING THEM
RU2012133852A
SHIKHTA AND METHOD OF ALUMINOTHERMIC PRODUCTION OF FERROTITANIUM WITH ITS USE
RU2015127577A
Method for preparing titanium alloys based on aluminothermic self-propagating gradient reduction and slag-washing refining
US20190241994A1