420MPa-grade sea wave splash zone corrosion resistant hot rolled strip steel for building structure and manufacturing method of 420MPa-grade sea wave splash zone corrosion resistant hot rolled strip steel

Through the design of low-carbon microalloy composition and hot-rolled strip steel without isolation layer combined with titanium and carbon steel, the corrosion resistance and mechanical properties of the steel structure in the environment of wave splash zone are solved, and high yield strength and tensile strength are achieved and low-temperature impact toughness improve the applicability and durability of steel structural parts.

CN119020685AActive Publication Date: 2024-11-26BAOSHAN IRON & STEEL CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202310604565.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

The prior art is difficult to provide building steel structures with materials that are both corrosion-resistant and have good mechanical properties in the environment of wave splash zones, especially the impact toughness and yield-strength ratio requirements under low temperature conditions are difficult to meet.

Method used

Designed with low-carbon microalloy composition, the thickness of the interface transition layer is controlled by combining titanium and carbon steel without adding metal isolation layer, and optimized through specific heating and rolling processes to form high yield strength and tensile strength. and low-temperature impact toughness for building structures.

Benefits of technology

It realizes that without reducing the corrosion resistance of the corrosion resistance layer, the mechanical properties of the base carbon steel meet the requirements of high strength grades, and have excellent yield and strength ratio and low temperature impact toughness. It is suitable for steel structural parts in the environment of the wave splash zone. , improves the applicability, safety and durability of components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020685A_ABST
    Figure CN119020685A_ABST
Patent Text Reader

Abstract

The invention discloses 420 MPa grade sea wave splashing zone corrosion resistant hot rolled strip steel for a building structure and a manufacturing method thereof. The hot rolled strip steel comprises a base layer, a corrosion resistant layer and an interface transition layer between the base layer and the corrosion resistant layer. The base layer is prepared from the following components in percentage by mass: 0.03 to 0.15 percent of C, 0.15 to 0.35 percent of Si, 1.0 to 1.5 percent of Mn, 0.0005 to 0.003 percent of P, 0.0005 to 0.01 percent of S, 0.08 to 0.45 percent of Cr, 0.08 to 0.60 percent of Ni, 0.05 to 0.2 percent of Cu, 0.02 to 0.05 percent of Al, 0.009 to 0.016 percent of Ti, 0.03 to 0.06 percent of Nb, 0.0005 to 0.005 percent of N, 0.08 to 0.25 percent of V and the balance of Fe and inevitable impurities; the corrosion-resistant layer is made of industrial pure titanium. According to the hot-rolled strip steel for the building structure, the yield strength is larger than or equal to 420 MPa, the tensile strength is larger than or equal to 570 MPa, the yield ratio is smaller than or equal to 0.79, the impact energy at the temperature of-40 DEG C is larger than or equal to 190 J, the wave splashing corrosion resisting rate is smaller than or equal to 0.006 mm / year, the thickness of an interface transition layer is smaller than or equal to 8 micrometers, and the interface shear strength is larger than or equal to 265 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel for building structures, and in particular to a hot-rolled steel strip for building structures resistant to corrosion in a sea wave splash zone and a manufacturing method thereof. Background Art

[0002] The ocean is a very harsh and complex corrosion environment. Seawater is a strong electrolyte solution containing high concentrations of chloride ions. Steel facilities, which are the main structures of marine engineering facilities, are very susceptible to electrochemical reactions with the surrounding media and are severely corroded, greatly reducing the service life of these facilities. Especially in the most demanding marine environmental corrosion area, the splash zone, various facilities are subject to a series of external factors such as alternating dry and wet conditions, seawater splashes, sunlight, corrosive components in the atmosphere, and oxygen, and the corrosion of materials is particularly serious.

[0003] Investigations show that steel piles in my country's seaports, offshore oil platforms and other facilities are severely corroded in this area, which is generally 3 to 10 times the area of ​​full seawater immersion. Once serious local corrosion damage occurs in this area, the bearing capacity of the entire facility will be greatly reduced, the service life will be shortened, production safety will be affected, and even the facility will be scrapped prematurely.

[0004] In the wave splash zone, due to the dry and wet alternating zone, the oxygen supply is sufficient, and the corrosion products produced have no protective effect; due to the splash of seawater, its droplets can directly hit the metal surface, causing serious corrosion. Corrosion tests and survey results show that under normal circumstances, the average corrosion rate of ordinary carbon steel, low alloy steel, etc. in the marine atmosphere is about 0.03-0.08 mm / year, while in the wave splash zone it is 0.3-0.5 mm / year. In the wave splash zone, this part is prone to serious corrosion damage, which greatly reduces the bearing capacity of the entire steel structure and affects safe production, shortens the service life, and scraps it in advance.

[0005] According to the above working conditions, industrial pure titanium is selected as the corrosion-resistant layer. Titanium has high chemical activity and easily reacts with oxygen in the air to form oxides. The oxides on the surface of titanium metal are dense, stable, and have strong "self-healing" ability. The "self-healing" ability of titanium oxide mainly refers to the fact that after the titanium oxide film at a certain place on the surface of titanium is damaged, it can quickly generate a new titanium oxide film to prevent further contact between corrosive media and titanium.

[0006] For marine building structure steel, in addition to meeting the requirements of corrosion resistance, it must also have good mechanical properties. Among them, the yield ratio and low-temperature impact toughness are increasingly becoming the key indicators of construction steel. The yield ratio is the ratio of the yield strength of steel to the tensile strength, and its size reflects the ability of steel to not produce strain concentration during plastic deformation. The lower the yield ratio, the more evenly the plastic deformation of the steel can be distributed over a wider range. Under the action of seismic force, the plastic deformation of the steel structure system made of low yield ratio steel can be evenly distributed over a wider range; while materials with high yield ratio may cause strain concentration, reducing the overall plastic deformation ability of the steel, resulting in brittle failure of the structure, causing the structure to freeze and suddenly collapse. Steel will undergo a brittle transition in a low temperature environment, and the fracture form of the steel will change from ductile fracture to brittle fracture. Its engineering significance lies in the fact that when the steel is in service at a temperature higher than this, the components will not undergo brittle fracture. Therefore, structural steel usually needs to make corresponding requirements for the low-temperature impact performance of steel according to the service environment of the material. The ocean temperature at different latitudes varies greatly. For example, near the Bohai Bay in China, the seaside temperature can reach below -20℃ in winter, which requires building materials to meet the impact performance of -40℃ to ensure that brittle fracture does not occur. If the increase in tensile strength is small while the material improves plastic toughness, the yield strength ratio will increase significantly, and the control of low yield strength ratio becomes difficult.

[0007] Chinese patent CN201210260231.7 discloses a method for preparing a titanium-steel-titanium double-sided composite plate, which comprises stacking four titanium plates and three steel plates in a certain order in a closed frame welded by two outermost steel plates, adding an isolating agent mixed with 1 part by weight of active α-Al2O3 and 1.5 parts by weight of a 4% polyvinyl alcohol aqueous solution between the titanium plates, and using a nickel-based alloy as a transition layer between the titanium plate and the steel plate, heating to 500°C to 630°C and evacuating, keeping warm for 1 to 2 hours, and achieving a vacuum degree of 20 to 200 Pa. The method is characterized by: After the billet is assembled, welding is first carried out and then vacuum is drawn. During welding, ordinary arc welding and submerged arc welding are sufficient. Compared with welding under vacuum conditions, the welding conditions are less demanding, the cost is low, and there is no need to set up a vacuum chamber separately. Subsequently, the assembled billet is rolled and compounded in a conventional heating furnace at a rolling temperature of 700°C to 900°C. The C in the coal gas can be isolated by sealing the outermost steel plate and vacuuming. At the same time, a nickel-based alloy isolation layer is added to prevent the formation of TiC on the interface, thereby obtaining a titanium-steel composite plate with a shear strength of 230 to 260 MPa and an interface bonding rate of 99.6% to 100%.

[0008] Chinese patent CN201710769999.X discloses a method for preparing a titanium-steel composite plate, which comprises selecting the surfaces of titanium-steel composite billets in contact with each other, applying a high-temperature resistant anti-carburizing and anti-nitriding isolation coating on the contacting titanium surfaces, and drying them at room temperature; after the drying process is completed, the titanium billets are aligned and stacked in pairs, and a steel billet is placed in the middle to complete the assembly to obtain a composite billet, wherein the thickness of the titanium plate used is greater than 2 mm, and the thickness of the steel plate is greater than 5 mm, and then the composite billet is sealed and welded around and a certain size of unwelded is left, and the billet is vacuumed to 10 -2 ~10 -3 Pa and then weld; heat the slab to 500-700℃ and roll it, the first pass reduction is more than 25%, the last pass reduction is no more than 15%, the total reduction is 60-70%, and the rolling speed is 0.1-1.0mm / s. The patent adopts a coating with high-temperature anti-seepage protection, which is protected from the diffusion and oxidation of other impurity elements at high temperatures, and blocks the diffusion of elements such as C and N. Its embodiment uses Q235 combined with TA1, and the shear strength of the produced steel plate reaches 176MPa, 181MPa, and 182MPa.

[0009] The above two patents mainly avoid the formation of brittle Ti compounds by adding an additional nickel-based alloy isolation layer between titanium and carbon steel.

[0010] Chinese patent CN201811327623.4 discloses a titanium-steel-titanium composite plate and a preparation method thereof. A carbon steel is fixed between two titanium plates of the same size, and warm composite rolling is performed by an irreversible large rolling force warm rolling mill to composite the three layers of strips into one. After rolling, the rolled composite plate is heat treated, including initial annealing at 500-600°C for 20-60 minutes and recrystallization annealing at 680-700°C for 30-120 minutes. Finally, the product is obtained by straightening, flattening, shearing and shaping. The patent mainly describes a preparation method for a non-hot-rolled composite titanium steel plate. Due to the use of an irreversible rolling mill, only a single-pass rolling production can be carried out, and heat treatment is also required. The embodiment mainly involves the steel strip production method, and the performance after composite is not mentioned.

[0011] Chinese patent CN201510543767.3 discloses a method for preparing a titanium-steel composite plate. The titanium-steel composite plate obtained by this method has high bonding strength. The patent fixes a titanium plate between two ordinary carbon steel plates or steel billets, welds the billets around in a vacuum environment, heats the combined billets to 850-900°C for 120-360 minutes, controls the starting rolling temperature to be above 800°C, and the final rolling temperature to be below 700°C, and controls the single-pass deformation to be 20-30%, and the total rolling deformation to be ≥90%. Large reduction rolling is performed to break the brittle phase compounds generated at the interface and reduce their influence on the bonding surface, and a titanium-steel composite plate with a bonding strength greater than 240MPa is obtained by rolling. The patent requires high reduction and total deformation per pass, and cracking of the edge weld is likely to occur during the rolling process, destroying the vacuum degree, and making the interface bonding unsuitable.

[0012] Chinese patent CN201610994234.1 discloses a production method of titanium-steel composite plate, which relates to an annealing technology production method of titanium-steel plate. First, titanium plate and steel plate are assembled to form a symmetrical multi-layer composite blank of steel plate-titanium plate-isolator-titanium plate-steel plate, which is compounded by rolling compounding or explosive compounding. The compounded blank is annealed and pickled in a continuous annealing and pickling line, first heated to 500-750°C to recrystallize the core titanium plate, and then heated to 950-1050°C to recrystallize the base steel plate. The purpose of this patent is to simultaneously obtain the properties of the composite material and the substrate through a two-stage heat treatment. The two-stage heat treatment will cause excessive diffusion of titanium, iron and carbon elements, produce brittle intermetallic compounds of iron and titanium carbide, and deteriorate the interface shear strength.

[0013] Chinese patent CN201710996925.X discloses a thin-layer double-sided titanium-steel composite plate and its preparation method. Through large-thickness blanking and large-reduction rolling technology, good composite between titanium and steel is achieved. The patent is a double-sided titanium composite plate composed of a titanium composite layer, a base layer and a titanium composite layer. The titanium composite layer is made of TA2, wherein the thickness of the titanium composite layer is 0.2 to 1 mm. The blanks are stacked in the middle in the order of cover plate, titanium composite material, carbon steel substrate, titanium composite material, and cover plate from top to bottom. After vacuum is drawn in a vacuum chamber, vacuum electron beam sealing welding is performed on the gaps around it, and the vacuum degree is 1.0 to 4.5×10 -2Pa, heat the sealed and welded composite billet to 900-920℃ for insulation, the insulation time is calculated according to 1min / mm×total thickness of the composite billet, the starting rolling temperature is 880-900℃, the final rolling temperature is above 800℃, air-cooled to room temperature, the single-pass reduction rate is ≥15%, and the first three-pass reduction rate is ≥20%, the total reduction rate is ≥80%, and the composite plate obtained after rolling is trimmed, split, and surface ground to obtain a double-sided titanium-steel composite plate. This patent achieves double-sided titanium-steel composite plates by surface cleaning of the composite billet, air isolation by the covering of the cover plate, control of the rolling temperature, and large reduction, so that the titanium-iron and titanium-carbon compounds generated at the composite interface are broken and refined, dispersed at the composite interface, and the distribution state of the compounds is improved, further ensuring the composite quality and performance stability, and the shear strength reaches 241MPa.

[0014] Chinese patent CN201710983322.6 discloses a thin composite titanium steel plate and a preparation method thereof, which adopts a double-layer structure of titanium and carbon steel. Its assembly method and heating process are similar to those of Chinese patent CN201710996925.X. The starting rolling temperature is 880-900°C, the single-pass reduction rate is 25-30%, and the total reduction rate is ≥85%. While controlling the single-pass reduction rate and the total reduction rate, the thickness of the titanium steel composite plate is limited to 3-16 mm, the final rolling temperature is above 800°C, and it is air-cooled to room temperature. The titanium steel composite plate is obtained by surface treatment, and the thickness of the titanium composite layer is ≤1 mm. This patent improves the composite quality by symmetrical assembly and welding titanium seals into carbon steel plates. After rolling, the shear strength of the steel plate reaches more than 238 MPa, and the composite interface bonding rate is 100%. Its carbon steel layer meets the national standard requirements for Q420 grade carbon steel.

[0015] The above two patents do not mention the detailed design of the composite layer and the base layer, but only describe the tensile properties and shear strength. The required pass reduction rate and total reduction rate of the composite layer are both relatively high, and there is no control over the corrosion resistance of the material, the low-temperature impact performance of the base material, the yield strength ratio and other performance indicators, which do not meet the requirements for steel used in building structures.

[0016] In summary, the above patents mainly describe the preparation method of the composite steel plate, and the specific embodiments mainly briefly describe the interface shear strength and tensile properties in terms of performance. In addition to being resistant to corrosion in the wave splash zone, the steel used for steel structures in the wave splash zone must also ensure that they have the necessary structural steel performance requirements, such as the aforementioned low yield ratio and corresponding low-temperature impact performance to ensure structural safety. However, the above patents have not carried out relevant component and process design for the corrosion rate, yield ratio, low-temperature impact, etc. of the corrosion-resistant layer, and cannot guarantee that the use requirements of high-corrosion-resistant steel plates for steel structures in the wave splash zone environment can be met. Summary of the invention

[0017] The object of the present invention is to provide a 420MPa grade hot-rolled steel strip for building steel structures resistant to sea wave splash zone corrosion and a manufacturing method thereof, wherein the mechanical properties of the base layer (carbon steel) can meet the corresponding strength level requirements without reducing the corrosion resistance of the corrosion-resistant layer itself, and the base layer has excellent yield strength ratio and low-temperature impact toughness; the yield strength of the hot-rolled steel strip for building structures is ≥420MPa, the tensile strength is ≥570MPa, the yield strength ratio is ≤0.79, the impact energy at -40°C is ≥190J, the sea wave splash corrosion rate is ≤0.006mm / year, the thickness of the interface transition layer is ≤8μm, and the interface shear strength is ≥265MPa; it can meet the corrosion resistance requirements in the sea wave splash zone environment, has good mechanical properties resistant to sea wave splash zone corrosion and high economy, and can be suitable for steel structural parts such as steel piles of facilities such as seaport terminals and offshore oil production platforms.

[0018] To achieve the above object, the technical solution of the present invention is:

[0019] The present invention adopts a low-carbon micro-alloying component design, and achieves an excellent combination of titanium and carbon steel without adding a metal isolation layer. At the same time, the thickness of the interface transition layer is controlled. Without reducing the corrosion resistance of the corrosion-resistant layer itself, the mechanical properties of the base layer (carbon steel) can also meet the corresponding strength level requirements, and the base layer has excellent yield strength ratio and low-temperature impact toughness.

[0020] Specifically, the 420MPa-grade hot-rolled steel strip for building structures resistant to sea wave splash zone corrosion of the present invention comprises a base layer, a corrosion-resistant layer, and an interface transition layer between the base layer and the corrosion-resistant layer;

[0021] The chemical composition mass percentage of the base layer is: C 0.03-0.15%, Si 0.15-0.35%, Mn 1.0-1.5%, P 0.0005-0.003%, S 0.0005-0.01%, Cr 0.08-0.45%, Ni 0.08-0.60%, Cu 0.05-0.2%, Al 0.02-0.05%, Ti 0.009-0.016%, Nb 0.03-0.06%, N 0.0005-0.005%, V 0.08-0.25%, and the balance includes Fe and other inevitable impurities;

[0022] The corrosion-resistant layer is made of industrial pure titanium;

[0023] The hot-rolled strip steel for building structures has a yield strength of ≥420MPa, a tensile strength of ≥570MPa, a yield strength ratio of ≤0.75, an impact energy at -40°C of ≥190J, a wave splash corrosion resistance rate of ≤0.006mm / year, an interface transition layer thickness of ≤8μm, and an interface shear strength of ≥265MPa.

[0024] Preferably, the chemical composition of the base layer also satisfies the following relationship:

[0025] 0.20%≤Cu+Ni≤0.75%;

[0026] 2(C+N)≤Ti+Nb+Cr+V≤0.60%.

[0027] Furthermore, the balance of the base layer components is Fe and other inevitable impurities.

[0028] The microstructure of the base layer of the present invention is ferrite+bainite+martensite, the content of bainite+martensite is 5-15%, and the average grain size of ferrite is ≥8.5.

[0029] The yield strength of the base layer of the present invention is ≥420MPa, the tensile strength is ≥570MPa, the yield strength ratio is ≤0.75, and the impact energy at -40°C is ≥190J.

[0030] Preferably, the corrosion-resistant layer is made of TA1, TA2, TA3 or TA4.

[0031] The microstructure of the corrosion-resistant layer is single, equiaxed α-Ti.

[0032] The sea wave splash corrosion resistance rate of the corrosion resistant layer is ≤0.006mm / year.

[0033] Preferably, the interface transition layer achieves 100% metallurgical bonding, the atoms are highly coherent, the thickness of the interface transition layer is ≤8 μm, and the interface shear strength is ≥265 MPa.

[0034] Preferably, the interface transition layer has fine grains, an average grain size of 15 to 40 μm, and contains (Ti, Nb)C precipitated particles smaller than 120 nm.

[0035] Preferably, the thickness of the hot-rolled steel strip for building structure is 1.0 to 20 mm.

[0036] In the base composition design of the hot-rolled strip steel for building steel structure of the present invention:

[0037] C: It plays a role of solid solution strengthening in steel and can significantly improve the strength of steel. However, too high C content is not good for welding performance and toughness. More importantly, too high C content will diffuse to the composite interface, forming a large number of large granular TiC hard phases in the interface transition layer, reducing the composite interface strength. In order to ensure the shear strength of the interface, the present invention adopts a low C content. The change of C content has less impact on the yield strength of steel than on the tensile strength. Under the premise of ensuring product molding and welding performance, appropriately increasing the C content is conducive to reducing the yield strength ratio of steel. Based on this, the C content in the base component described in the present invention is controlled at 0.03-0.15%.

[0038] Si: Adding Si to steel can effectively deoxidize and improve the purity of steel. In addition, Si can play a role in solid solution strengthening in steel, which can improve the strength and hardness of steel, but Si is not conducive to the welding performance of the material. Therefore, the Si content in the base composition of the present invention is controlled to be 0.10-0.30%.

[0039] Mn: Mn is the cheapest matrix strengthening element, which can reduce the austenite transformation temperature, delay the pearlite transformation, refine the ferrite grains, and improve the strength of steel. At the same time, Mn can also eliminate the influence of S on steel. However, if the Mn content is too high, segregation bands and martensite structures are likely to appear, which is not good for the toughness of steel. Therefore, the Mn content in the base composition of the present invention is controlled to be 1.0% to 1.5%.

[0040] Al: Al is mainly added to the steel as an element for removing O in excess to ensure that the O content in the steel is as low as possible. After removing O, the excess Al combines with the N element in the steel to form AlN precipitates. AlN hinders the growth of austenite grains during heating, refines austenite grains, and improves matrix strength and toughness. At the same time, the formation of AlN fixes part of the N in the matrix, reduces the diffusion of interstitial atomic N in the carbon steel base layer to the composite interface, forms hard TiN in the interface transition layer, and deteriorates the interface shear strength of the composite plate. At the same time, the addition of Ti and Nb can be reduced, reducing the total cost. Based on this, the Al content in the base composition of the present invention is controlled to be 0.015-0.03%.

[0041] Ti: Ti forms stable TiN or Ti(N, C) at high temperature, which plays a role in fixing C and N, preventing interstitial C and N atoms in the carbon steel base from diffusing to the interface, and forming hard TiN or Ti(N, C) precipitation in the interface transition layer to obtain a composite plate with high interface shear strength. At the same time, TiN hinders the growth of austenite during heating, refines austenite grains, and improves matrix strength and toughness. In subsequent welding, especially in the heat affected zone (HAZ) close to the molten boundary of the weld, the growth of austenite grains is inhibited, thereby improving the toughness of the welding HAZ, and being able to meet the needs of large welding heat input processes. In order to improve the strength of the low-carbon matrix and reduce the diffusion of C and N to the interface, a composite plate with high interface shear strength is obtained. Based on this, the Ti content in the base component of the present invention is controlled to be 0.009-0.016%.

[0042] Nb: Nb exists in the steel in the form of solid solution Nb and Nb(C, N), and plays the role of solid solution dragging and precipitation pinning during the recrystallization process. A small amount of Nb is added to the base carbon steel mainly to increase the recrystallization temperature, so that the base carbon steel can be refined after rolling in the recrystallization and non-recrystallization zones, which is beneficial to improving the low-temperature impact toughness of the base carbon steel. Due to the precipitation phase effect of Nb(C, N), the original austenite grains will be finer, thereby promoting the formation of finer recrystallized grains and obtaining an ideal combination of high strength and high toughness. At the same time, Nb can fix the interstitial C and N atoms in the matrix, reduce the diffusion of C and N to the interface, and obtain a composite plate with high interface shear strength. Based on this, the Nb content in the base layer described in the present invention is controlled to be 0.030-0.06%.

[0043] Cu: Cu plays a role in solid solution strengthening, and as the Cu content increases, the room temperature impact toughness of the steel slightly increases. Therefore, the Cu content in the base layer component of the present invention is controlled to be 0.050-0.20%.

[0044] N: The N element can generate second phase particles with Ti and Al, refine austenite grains, and improve matrix strength and toughness. However, when the N content is too high, the amount of TiN generated is large and the particles are too coarse, which will affect the plasticity and toughness of the base carbon steel of the present invention. Based on this, the N content in the base of the present invention is controlled to be 0.0005-0.005%.

[0045] Ni: Ni is an element that stabilizes austenite and has a certain effect on improving toughness and strength. Adding Ni to steel can greatly improve the low-temperature impact toughness of steel. However, nickel is expensive, and excessive addition will increase the cost of the composite plate. Based on this, an appropriate amount of Ni is added to the base component of the present invention, and the Ni content is controlled to 0.08-0.60%.

[0046] Cr: Cr is a strong carbide-forming element, which has a low diffusion rate in austenite and hinders the diffusion of C element. It forms fine carbides in the low temperature process, which plays a role of precipitation strengthening. At the same time, it can fix the interstitial C and N atoms in the matrix, reduce the diffusion of C and N to the interface, and obtain a composite plate with high interface shear strength. Cr in steel increases the strength of the matrix while reducing toughness. In order to obtain the best match between strength and toughness, the Cr content in the base component of the present invention is controlled at 0.08-0.45%.

[0047] V: V is a strong carbonitride-forming element. When added in combination with Ti and Nb in steel, it can form fine composite carbonitrides, and the precipitation temperature range becomes wider, which can effectively organize the growth of austenite grains, inhibit the recrystallization process, and improve the strength and toughness of the base carbon steel. At the same time, the precipitation temperature of V carbonitride is relatively low, and the precipitation during the phase transformation process can effectively organize the growth of ferrite grains and strengthen the strength of the ferrite matrix. Based on this, an appropriate amount of V is added to the base component of the present invention, and the V content is controlled to 0.08-0.25%.

[0048] S and P are both inevitable impurity elements, and their contents should be as low as possible. Considering the actual steelmaking level of the steel plant, the S and P contents are controlled as follows in the present invention: S≤0.010%; P≤0.003%;

[0049] The corrosion-resistant layer of the present invention adopts industrial pure titanium, preferably TA1, TA2, TA3 and TA4, and its composition meets the standard of GB / T3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Compositions".

[0050] In addition, in the base chemical composition design of the hot-rolled strip steel for building steel structure of the present invention:

[0051] Since both Cu and Ni can improve the toughness of the base layer, and the composite addition effect is particularly significant, at the same time, the addition of Ni element can reduce the diffusion rate of C in steel and reduce the diffusion of C to the interface. Therefore, the present invention controls 0.20%≤Cu+Ni≤0.75%, and can control the interface transition layer within 8μm.

[0052] Since Ti, Nb, Cr and V are all strong carbonitride forming elements, corresponding carbonitrides will be formed in the base carbon steel, which can fix the interstitial atoms in the base, hinder the diffusion of C and N interstitial atoms to the interface, and form large particles and aggregated carbonitrides in the interface transition layer, which can control the interface transition layer within 8μm, thereby improving the interface shear strength. At the same time, Ti, Nb and Cr can play a role in refining the base carbon steel grains and improving toughness at different stages of hot rolling. Therefore, the present invention controls: 2(C+N)≤Ti+Nb+Cr+V≤0.60%.

[0053] The method for manufacturing the 420MPa-grade hot-rolled strip steel for building structures resistant to sea wave splash zone corrosion of the present invention comprises the following steps:

[0054] 1) Smelting and casting

[0055] According to the composition of the base layer and the corrosion-resistant layer, they are smelted and cast into billets respectively;

[0056] 2) Assembly

[0057] The base layer and the corrosion-resistant layer blanks are ground and polished, and the bonding surfaces of the blanks are welded and sealed all around to form a composite blank; the bonding surfaces after welding and sealing are vacuumed;

[0058] 3) Heating

[0059] Heating the composite blank to 900-1000° C.;

[0060] 4) Rolling

[0061] The rough rolling temperature is controlled above 860℃; the finishing rolling temperature is controlled at 780℃~850℃, the pass reduction rate is controlled at 5~20%, and the cumulative reduction rate is ≥88%;

[0062] 5) Cooling

[0063] In the first stage, the steel strip is cooled to 700~750℃ at a cooling rate of ≤10℃ / s after leaving the rolling mill.

[0064] ℃, and then in the second stage, it is cooled to 350-450℃ at a cooling rate of 30-50℃ / s for coiling.

[0065] Preferably, the thickness of the corrosion-resistant layer in step 1) is 1 to 10% of the total thickness of the composite blank.

[0066] Preferably, the rolling reduction rate used in step 4) is 10-15%.

[0067] In the manufacturing method of the present invention:

[0068] 1) Smelting: P and S elements will deteriorate the fracture toughness of steel, so low P and low S should be controlled during the smelting process to improve the quality of the steel billet. Clean steel production technology is used to reduce the gas and inclusion content in the steel, improve the comprehensive performance of the steel, especially the anti-lamellar tearing performance.

[0069] 2) Assembly; the thickness of the corrosion-resistant layer is prepared according to 1-10% of the total thickness of the composite billet. The corrosion-resistant layer and the base carbon steel billet are pretreated, and the billet bonding surface is welded and sealed all around, and the bonding surface after welding and sealing is vacuumed. The vacuum treatment protects the surface of the corrosion-resistant layer from oxidation, and is also an important condition to ensure that the corrosion-resistant layer is resistant to corrosion in the splash zone. At the same time, it can ensure that the corrosion-resistant layer avoids edge cracking and corrosion-resistant layer rolling during the subsequent large cumulative reduction rate deformation process.

[0070] 3) Heating: For single carbon steel, the slab heating temperature is generally controlled at 1000-1250°C, which is conducive to the dissolution and full diffusion of precipitates in the steel, promotes the homogenization of slab elements, and exerts the strengthening effect of microalloying elements in the steel; for a single industrial pure titanium plate, the heating temperature is generally controlled at 850-1000°C. If the heating temperature is too high, β phase transformation will occur, and the β phase will grow rapidly, deteriorating the performance of industrial pure titanium, because the heating temperature is too high and the elements will also be fully diffused, promoting the subsequent realization of 100% metallurgical bonding of the interface; but higher heating temperatures will increase the tendency of austenite grains to coarse, increase the difficulty of subsequent controlled rolling, and most importantly, accelerate the diffusion of C, N, Ti, and Fe to the interface, forming thicker brittle precipitates and intermetallic compounds at the interface, forming a thick interface transition layer, and deteriorating the interface shear strength. Preferably, a relatively low heating temperature is used for traditional carbon steel production, and the heating temperature is set to between 900 and 1000°C.

[0071] 4) Rolling: The rough rolling temperature is controlled at above 860℃. In the high temperature rough rolling zone, a large reduction rate is applied to fully recrystallize the structure, refine the grains, and improve the strength and toughness of the material. In the non-recrystallized zone of fine rolling, controlled rolling is applied. Austenite recrystallization no longer occurs at this stage. The deformation energy and deformation dislocation are accumulated through a reasonable reduction rate and final rolling temperature, so that a high-density deformation band is formed inside the austenite grains, the ferrite phase deformation nuclei are increased, and the grain size after the matrix phase transformation is further refined, and the material strength and toughness are improved. At the same time, at this stage, deformation induces the precipitation of carbonitrides of Nb, Ti, Cr and V, which improves the strength of the matrix, inhibits the diffusion of C to the interface, and avoids the formation of too thick TiC at the interface to deteriorate the interface shear strength. The pass reduction rate is guaranteed to be 5-20%, and the cumulative reduction rate is ≥88%; preferably, the finishing temperature is controlled at 780°C-850°C, while ensuring the corrosion resistance of titanium, avoiding the base layer from rolling in the two-phase region, and obtaining ferrite with an average grain size of ≥8.5 and a bainite + martensite structure with a content of 5-15%.

[0072] 5) Cooling: By controlling the initial cooling, final cooling and cooling speed, the type, size and content of the rolled structure can be controlled. Too fast cooling will form a large amount of bainite and martensite structures. Since the martensite phase is a low-toughness and high-yield ratio structure, it is not good for the performance of the steel plate. Too slow cooling will lead to the formation of a large amount of coarse ferrite structure. The coarse structure is beneficial to the expansion of cracks, resulting in a decrease in impact performance. Therefore, the cooling rate should be reasonably controlled; the control of the finishing rolling temperature can avoid the abnormal coarse structure caused by rolling in the two-phase region; at the same time, it can be quickly cooled to the phase transition temperature after rolling, further inhibiting the growth of the structure, improving the material strength and low-temperature impact toughness by refining the grains, and forming more than 5% of the hard phase structure to ensure strength. Preferably, a two-stage cooling method is adopted. After leaving the rolling mill frame, it is first cooled to the ferrite phase transformation temperature at a cooling rate of ≤10°C / s, and then quickly cooled to 350-450°C at a cooling rate of 30-50°C / s for coiling to obtain a small amount of bainite and martensite structures. In addition, during the coiling process, the structure recovery is achieved, and the precipitation of V carbonitride is promoted, ensuring that the base layer has a low yield strength ratio and high low-temperature impact toughness.

[0073] Preferably, when the corrosion-resistant layer is too thick, it will affect the mechanical properties and production cost of the material; and when the corrosion-resistant layer is too thin, it will reduce the corrosion resistance and service life of the material. For this reason, the ratio of the corrosion-resistant layer in the above-mentioned assembly process to the total thickness of the composite blank is preferably 1-10%.

[0074] The present invention composites the corrosion-resistant layer with the base layer, combines the component design and the thickness ratio design of the two, and forms a corrosion-resistant layer resistant to sea wave splash zone corrosion on the base layer, i.e., the surface of the carbon strip steel, through a rolling process, ultimately forming a strip steel that has sea wave splash zone corrosion resistance, good mechanical properties and high economy. The strip steel can be further processed into structural parts that can be effectively used in steel structural parts for use in sea wave splash zone environments.

[0075] Compared with the prior art, the present invention has the following beneficial effects:

[0076] The present invention adopts a low-carbon micro-alloying component design, and achieves an excellent combination of titanium and carbon steel without adding a metal isolation layer. At the same time, the thickness of the interface transition layer is controlled. Without reducing the corrosion resistance of the corrosion-resistant layer itself, the mechanical properties of the base layer (carbon steel) can also meet the corresponding strength level requirements, and the base layer has excellent yield strength ratio and low-temperature impact toughness.

[0077] The present invention adopts a low-C micro-alloy design, and reduces the formation of TiC compounds in the interface transition layer and the formation of carbonitrides in the base layer by reducing C, thereby hindering grain growth and improving the low-temperature impact toughness of the base layer. At the same time, the addition of micro-alloy elements and a reasonable rolling cooling process solve the problem of low material strength under low-carbon conditions. The yield strength is ≥420MPa, the tensile strength is ≥570MPa, and the material yield strength ratio is ≤0.79, and the -40°C impact energy is ≥190J, both of which are higher than the performance requirements of the national standard GB / T19879-2015 "Steel Plates for Building Structures".

[0078] Chinese patent CN201210260231.7 does not specify the heating temperature. By adding a nickel plate as an isolation layer between the composite layer and the base layer to prevent the formation of interface TiC, the interface bonding rate of the titanium steel composite plate is 99.6-100%. The present invention specifies that the heating temperature of the composite billet is 900-1000°C, and through low-carbon and micro-alloy design, the addition of Ni is reduced, and the production cost is reduced. At the same time, through the optimization of heating, rolling and other process processes, a transition layer structure of a certain thickness can be formed, and the formation of brittle phase TiC in the interface transition layer is reduced, achieving a complete metallurgical bonding with an interface bonding rate of 100%.

[0079] The heating temperature of the slab in Chinese patent CN201710769999.X is 500-700℃, the total reduction rate is 60-70%, and the maximum interface shear strength of the produced strip is 182MPa. The present invention fully considers the influence of the high-temperature phase transformation of industrial pure titanium in the corrosion-resistant layer on the corrosion resistance and the strength and toughness control of the base carbon steel. Combined with the low-carbon microalloy design and the global design of the processing technology, the heating temperature of the composite billet is set to 900-1000℃. At this temperature, the corrosion-resistant layer does not undergo phase transformation, and the precipitates in the base carbon steel are fully dissolved. In the controlled rolling process, the base grains are refined to improve the base strength and toughness. Combined with the cumulative reduction rate ≥85%, the brittle phase of the interface transition layer is broken and the interface shear strength is improved.

[0080] The above two patents mainly avoid the formation of brittle Ti compounds by adding an additional nickel-based alloy isolation layer between titanium and carbon steel, while the present invention does not add an isolation layer through composition and process design, and has a different assembly method from the above two patents and a significantly different material of the base carbon steel.

[0081] Under the process conditions of the present invention, both the original corrosion resistance of the industrial pure titanium of the corrosion-resistant layer and the mechanical properties of the base layer are guaranteed, solving the problem that the two processing windows of traditional titanium and carbon steel are too different to be taken into account; at the same time, the elements of the base layer and the corrosion-resistant layer are fully diffused to form an interface transition layer not larger than 10 μm. The layer has fine grains, an average grain size of 15 to 40 μm, and contains (Ti, Nb)C precipitated particles smaller than 120 nm, which strengthens the interface bonding performance and ensures that the interface shear strength is ≥265 MPa, which is higher than the interface shear strength of 182 MPa of Chinese patent CN201710769999.X.

[0082] Chinese patent CN201811327623.4 achieves compounding through warm rolling, followed by a two-stage heat treatment operation, including a primary annealing at 500-600°C for 20-60 min and a recrystallization annealing at 680-700°C for 30-120 min. It is a preparation method for a non-hot-rolled composite titanium strip steel, which is completely different from the manufacturing method of the present invention.

[0083] Chinese patent CN201510543767.3 has a heating temperature of 850-900°C, a final rolling temperature of 700°C or less, and controls the single-pass deformation to be 20-30%, the total rolling deformation ≥90%, and the shear strength of the titanium-steel composite plate is greater than 240MPa. The pass reduction and total deformation required by the patent are both very high, and the edge weld cracks easily occur during the rolling process, destroying the vacuum, not easy to composite, and poor rolling stability. The single-pass deformation of the present invention is controlled at 5-20%, which can effectively control the weld from cracking during the rolling process, ensure the vacuum inside the slab, and improve the interface shear strength and the stability and success rate of rolling.

[0084] Chinese patent CN201610994234.1 is a production method of annealing technology for titanium steel plate. First, titanium plate and steel plate are assembled to form a symmetrical multi-layer composite blank of steel plate-titanium plate-isolator-titanium plate-steel plate, which is compounded by rolling compounding or explosive compounding. The compounded blank is annealed and pickled by a continuous annealing and pickling line, first heated to 500-750°C to recrystallize the core titanium plate, and then heated to 950-1050°C to recrystallize the base steel plate. The rolling process and the corrosion and structural properties of the obtained steel plate are not specifically clarified. The present invention is obviously different from the present invention in terms of manufacturing process. The present invention does not need to perform two-stage heat treatment, and the two-stage heat treatment will cause excessive diffusion of titanium, iron and carbon elements, produce brittle intermetallic compounds of iron and titanium and titanium carbide, and deteriorate the interface shear strength.

[0085] The corrosion-resistant layer material of Chinese patent CN201710996925.X is TA2, in which the titanium composite layer is 0.2-1mm thick, heated to 900-920℃ for insulation, the start rolling temperature is 880-900℃, the final rolling temperature is above 800℃, air-cooled to room temperature, and the shear strength reaches 241MPa. The heating temperature of the present invention is 900-1000℃, the finishing rolling temperature is 750℃-850℃, and the cooling is carried out in two stages. Under this process, TA1, TA2, TA3 and TA4 can be used as corrosion-resistant layers, and the corrosion-resistant layer accounts for 0.5-20% of the total thickness of the composite billet, and the interface shear strength is ≥265MPa.

[0086] The assembly method and heating process of Chinese patent CN201710983322.6 are similar to those of Chinese patent CN201710996925.X. The single-pass reduction rate is 25-30%, and the total reduction rate is ≥85%. While controlling the single-pass reduction rate and the total reduction rate, the thickness of the titanium-steel composite plate is limited to 3-16 mm, the final rolling temperature is above 800°C, and air-cooled to room temperature. The titanium-steel composite plate is obtained by surface treatment, and the thickness of the titanium composite layer is ≤1 mm. The single-pass reduction rate of the present invention is 5-20%, the rolling stability is controlled, and a two-stage cooling method is adopted to ensure the organizational type of the material, thereby controlling the yield strength ratio and toughness. There are also obvious differences in the thickness of the corrosion-resistant layer and the total thickness of the composite strip.

[0087] The 420MPa-grade hot-rolled steel strip for building structures resistant to sea wave splash zone corrosion of the present invention can solve the essential pain points of stainless steel or carbon steel used in sea wave splash zone environment; the 420MPa-grade hot-rolled steel strip for building structures resistant to sea wave splash zone corrosion can be effectively applied to the manufacture of steel structural parts used in sea wave splash zone environment, for example: steel structural parts of facilities such as seaport terminals and offshore oil platforms in sea wave splash zone, which can meet the requirements of these components for sea wave splash zone corrosion resistance and mechanical properties, greatly improve the applicability, safety and durability of these components, and have great economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0088] Figure 1 This is a schematic diagram of an interlayer structure of the 420MPa grade hot-rolled strip steel for building structures resistant to sea wave splash zone corrosion according to the present invention.

[0089] Figure 2 This is another schematic diagram of the interlayer structure of the 420MPa grade hot-rolled strip steel for building structures resistant to sea wave splash zone corrosion according to the present invention.

[0090] Figure 3 This is a microstructure photograph of the corrosion-resistant layer of Example 3 of the present invention.

[0091] Figure 4This is a scanned image of the interface transition layer combining the base layer and the corrosion-resistant layer in Example 3 of the present invention.

[0092] Figure 5 This is a photo of the base layer microstructure of Example 3 of the present invention. DETAILED DESCRIPTION

[0093] The technical solution of the present invention is further described in detail below in conjunction with the examples and drawings. It should be clear that the following examples are only used to describe the specific implementation methods of the present invention and do not constitute any limitation on the protection scope of the present invention.

[0094] See also Figure 1 , Figure 2 , Figure 4 , which is a schematic diagram of the two interlayer structures of the hot-rolled strip steel for building structure according to the present invention, wherein 1 is the base layer, 2 is the corrosion-resistant layer, and 3 is the interface transition layer.

[0095] The composition of the base layer of the embodiment of the hot-rolled steel strip (composite steel plate) for building structure of the present invention is shown in Table 1, and the remainder of the composition is Fe and unavoidable impurities. Table 2 shows the manufacturing process parameters of the embodiment of the composite steel plate of the present invention. Table 3 shows the metallographic structure and mechanical properties of the base layer and the corrosion-resistant layer, and the thickness of the interface transition layer in the composite steel plates of the embodiments and comparative examples.

[0096] Among them, the yield strength and tensile strength of the composite steel plate are measured with reference to GB / T 6396-2008 "Methods for Mechanical and Process Properties of Composite Steel Plates" and GB / T 228-2010 "Room Temperature Tensile Test Methods for Metallic Materials".

[0097] The -40℃ impact energy KV2 / J (longitudinal) of the base carbon steel is measured in accordance with GB / T 6396-2008 "Mechanical and Processing Properties of Composite Steel Plates" and GB / T 229-2020 "Charpy Pendulum Impact Test Method for Metallic Materials".

[0098] The grain size rating is carried out as follows: According to GB / T 6394-2017 "Method for Determination of Average Grain Size of Metals", the intercept method is used to grade the grain size of ferrite in stainless steel and carbon steel respectively.

[0099] The comparative example is prepared by the above steps which are basically the same as those of the embodiment of the present invention, except that the composition of the base carbon steel and certain process parameters used in the rolling or cooling steps do not meet the requirements of the present invention.

[0100] The metallographic structure of the corrosion-resistant layer of Example 3 is shown in Figure 3 , showing a single, equiaxed α-Ti with an average grain size of 103.4um.

[0101] The interface transition layer of Example 3 is shown in Figure 4 The thickness of the interface transition layer 3 is 7.3 μm, in which the intermittent fine particles are TiC with a size less than 120 nm.

[0102] The base metallographic structure of Example 3 is shown in Figure 5 , showing that the metallographic structure of the base carbon steel is ferrite + bainite + martensite, the volume fraction of bainite + martensite is 9.1%, and the ferrite grain size grade is ≥8.5.

[0103] Table 4 shows the corrosion conditions of the composite steel plate coupon samples of Examples 1-8 and Comparative Examples 1-4 after 6 months in the wave splash zone of the South China Sea. The observation results show that, except for Comparative Example 4, the corrosion rates of the other Examples and Comparative Examples are all ≤0.006 mm / year.

[0104] Comparative Examples 1-4 use unsatisfactory composition design requirements and hot working process conditions, resulting in certain properties of the composite steel plate failing to meet the use requirements (performance parameters are not within the scope of the invention).

[0105] In Comparative Example 1, since the pass reduction rate and the cumulative reduction rate are not within the range specified by the present invention, the grains are coarse, and the yield strength and impact energy cannot meet the requirements.

[0106] Since the Cu+Ni addition amount in Comparative Example 2 is less than 0.2%, its impact performance cannot meet the requirements.

[0107] Since the coiling temperature of Comparative Example 3 is not within the range specified by the present invention, the yield strength ratio and impact properties cannot meet the requirements.

[0108] In Comparative Example 4, since no V element is added, the cooling speed after leaving the rack and the speed in the second stage cold zone are not within the scope specified by the present invention, and the necessary precipitation strengthening effect is lacking, and the yield strength and tensile strength thereof cannot meet the requirements.

[0109] In Comparative Example 5, since the heating temperature and the finishing rolling temperature are not limited in the present invention, the thickness of the transition layer increases and the shear strength cannot meet the requirements.

[0110] Through the preparation method of the present invention, especially the control of the heating, rolling and cooling processes, the base layer in the strip steel exhibits a low yield strength ratio and good low-temperature impact toughness, and the coating layer has excellent corrosion resistance and high bonding strength, with a yield strength of 430-508MPa, a tensile strength of 577-645MPa, a yield strength ratio of ≤0.79, an impact energy at -40°C of more than 190J, and an interface shear strength of more than 265MPa.

[0111] It should be noted that all technical features described in the present invention can be freely combined or combined in any way unless there is a contradiction between them. Various modifications and changes can be made to the present invention without departing from the scope of the present invention, which will be obvious to those skilled in the art. For example, a feature shown or described as part of one embodiment can be used together with another embodiment to produce another embodiment. Therefore, the present invention is intended to cover these modifications that fall within the scope of the appended claims and their equivalents.

[0112]

[0113]

[0114]

[0115]

[0116]

Claims

1. 420MPa grade hot-rolled steel strip for building structures resistant to sea wave splash zone corrosion, including base layer, corrosion resistant layer and interface transition layer between base layer and corrosion resistant layer; The chemical composition mass percentage of the base layer is: C 0.03-0.15%, Si 0.15-0.35%, Mn 1.0-1.5%, P 0.0005-0.003%, S 0.0005-0.01%, Cr 0.08-0.45%, Ni 0.08-0.60%, Cu 0.05-0.2%, Al 0.02-0.05%, Ti 0.009-0.016%, Nb 0.03-0.06%, N 0.0005-0.005%, V 0.08-0.25%, and the balance includes Fe and other inevitable impurities; The corrosion-resistant layer is made of industrial pure titanium, preferably TA1, TA2, TA3 or TA4; The hot-rolled strip steel for building structure has a yield strength of ≥420MPa, a tensile strength of ≥570MPa, a yield strength ratio of ≤0.79, an impact energy at -40°C of ≥190J, a wave splash corrosion resistance rate of ≤0.006mm / year, an interface transition layer thickness of ≤8μm, and an interface shear strength of ≥265MPa.

2. The hot-rolled steel strip for building structure according to claim 1, characterized in that: The chemical composition of the base layer also satisfies the following relationship: 0.20%≤Cu+Ni≤0.75%; 2(C+N)≤Ti+Nb+Cr+V≤0.60%.

3. The hot rolled steel strip for building structure according to claim 1 or 2, characterized in that: The balance of the base layer composition is Fe and other inevitable impurities.

4. The hot rolled steel strip for building structure according to claim 1, 2 or 3, characterized in that: The microstructure of the base layer is ferrite+bainite+martensite structure, the content of bainite+martensite is 5-15%, and the average grain size of ferrite is ≥8.

5.

5. The hot rolled steel strip for building structure according to claim 1, 2, 3 or 4, characterized in that: The yield strength of the base layer is ≥420MPa, the tensile strength is ≥570MPa, the yield strength ratio is ≤0.79, and the impact energy at -40°C is ≥190J.

6. The hot rolled steel strip for building structure according to claim 1, characterized in that: The microstructure of the corrosion-resistant layer is single, equiaxed α-Ti.

7. The hot rolled steel strip for building structure according to claim 1 or 6, characterized in that: The sea wave splash corrosion resistance rate of the corrosion resistant layer is ≤0.006mm / year.

8. The hot rolled steel strip for building structure according to claim 1, characterized in that: The interface transition layer achieves 100% metallurgical bonding, the atoms are highly coherent, the thickness of the interface transition layer is ≤8 μm, the grain size of the layer is fine, the average grain size is 15-40 μm, and contains less than 120nm (Ti, Nb)C precipitated particles, interface shear strength ≥265MPa.

9. The hot rolled steel strip for building structure according to claim 1, characterized in that: The thickness of the hot-rolled steel strip for building structure is 1.0-20 mm.

10. The method for manufacturing the 420MPa grade hot-rolled steel strip for building structures resistant to sea wave splash zone corrosion according to any one of claims 1 to 9, characterized in that: The steps include: 1) Smelting and casting The components of the base layer and the corrosion-resistant layer according to claim 1, 2 or 3 are smelted and cast into billets respectively; 2) Assembly The base layer and the corrosion-resistant layer blanks are ground and polished, and the bonding surfaces of the blanks are welded and sealed all around to form a composite blank; the bonding surfaces after welding and sealing are vacuumed; 3) Heating Heating the composite blank to 900-1000° C.; 4) Rolling The rough rolling temperature is ≥860℃, the finishing rolling temperature is controlled at 780~850℃, the pass reduction rate is controlled at 5~20%, and the preferred pass reduction rate is 10~15%; the cumulative reduction rate is ≥88%; 5) Cooling In the first stage, the steel strip is cooled to 700-750°C at a cooling rate of ≤10°C / s after leaving the rolling mill stand, and then in the second stage, it is cooled to 350-450°C at a cooling rate of 30-50°C / s for coiling.

11. The manufacturing method according to claim 10, characterized in that: Step 1) The thickness of the corrosion-resistant layer is 1 to 10% of the thickness of the composite blank.

Citation Information

Patent Citations

  • Manufacturing method of titanium-steel-titanium two-sided composite plate

    CN102773670A

  • Preparation method of titanium-steel clad plate

    CN105107841A

  • Production method of titanium-steel composite plate

    CN106269963A

  • Preparation method of titanium-steel composite plate

    CN107626764A

  • Titanium-steel-titanium composite plate and preparation method thereof

    CN109304367A