High-strength and high-corrosion-resistance super martensitic stainless steel as well as preparation method and application thereof

By controlling the content of elements such as C, Cr, Mo, Ni, and Cu and the preparation process, the problem of high cost of nickel-based alloys has been solved, and high-strength, high-corrosion-resistant super martensitic stainless steel has been developed to meet the needs of oil and gas fields for high-strength, high-corrosion-resistant materials, which are suitable for marine engineering.

CN119020704AInactive Publication Date: 2024-11-26GUANGDONG INST OF NEW MATERIALS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411143200.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In existing technologies, nickel-based alloy materials are expensive and their costs are rising, making it difficult to meet the needs of oil and gas fields for high-strength and high-corrosion-resistant materials. Traditional super martensitic stainless steel has not yet met the requirements for high strength and excellent corrosion resistance in oil well pipe material research.

Method used

By rationally selecting the content of elements such as C, Cr, Mo, Ni, and Cu, a high-strength and high-corrosion-resistant super martensitic stainless steel is prepared. The process involves steps such as smelting, homogenization, forging, and cooling to ensure that the stainless steel has a fully martensitic structure, thereby improving yield strength and tensile strength and reducing raw material costs.

Benefits of technology

The prepared super martensitic stainless steel has high yield strength and tensile strength, good electrochemical corrosion resistance, is suitable for industrial production, reduces material costs, is applicable to marine engineering, and has the potential to replace 316L stainless steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005001504030000111
    Figure BDA0005001504030000111
  • Figure BDA0005001504030000121
    Figure BDA0005001504030000121
  • Figure HDA0005001504040000011
    Figure HDA0005001504040000011
Patent Text Reader

Abstract

The invention discloses high-strength and high-corrosion-resistance super martensitic stainless steel, a preparation method and application, and the high-strength and high-corrosion-resistance super martensitic stainless steel comprises the following element components in percentage by mass: 0.02-0.04% of C, 12-18% of Cr, 0.5-2% of Mo, 4-8% of Ni, 0.5-1.5% of Cu, less than or equal to 0.02% of P, less than or equal to 0.02% of S and the balance of Fe. The preparation method comprises the following steps: S1, weighing raw materials according to a formula, smelting and pouring to obtain a steel billet; s2, the steel billet is subjected to first homogenization treatment and heat preservation, and a square billet is obtained; s3, the square billet is subjected to forging treatment, and a stainless steel crude product is obtained; and S4, the stainless steel crude product is subjected to second homogenization treatment, heat preservation and cooling, and the super martensitic stainless steel is obtained. The super martensitic stainless steel has higher yield strength and tensile strength and more excellent electrochemical corrosion resistance. In addition, the preparation method does not need secondary tempering, is simple in process, low in raw material cost and suitable for industrial production, and is applied to the field of ocean engineering to further reduce the cost of steel materials for ocean engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of martensitic stainless steel preparation, and particularly relates to a high-strength and high-corrosion-resistant super martensitic stainless steel, a preparation method and application thereof. Background Art

[0002] As the conditions for the exploitation of oil and natural gas become increasingly harsh, the performance requirements for service materials are also becoming more stringent. Based on the current exploitation status of oil and gas fields and the actual working conditions of major oil and gas fields, oil well pipes require high-strength and high-corrosion-resistant materials to ensure safe service in extremely harsh oil and gas fields. Due to their excellent mechanical properties and corrosion resistance, nickel-based alloy materials are imported in large quantities for the exploitation of domestic oil fields. However, this type of nickel-based alloy is expensive, causing domestic oilfield companies to bear a huge economic burden. With the rapid development of the battery industry, the price of Ni element raw materials has continued to rise, which in turn has caused a sharp increase in the cost of nickel-based alloys. Therefore, the development of high-strength and high-corrosion-resistant materials is a major material problem that needs to be urgently solved in the field of oil and gas field equipment.

[0003] Super martensitic stainless steel has received extensive attention, active exploration and certain applications in the fields of oil and gas transmission pipelines and offshore drilling platforms due to its high strength, good wear resistance, good creep resistance and excellent corrosion resistance. However, with the in-depth research on oil well pipe materials, oil and gas companies have put forward clear requirements for super martensitic stainless steel, such as higher strength and better corrosion resistance. The development of new high-strength and high-corrosion-resistant martensitic stainless steel to replace traditional nickel-based alloys is the hot spot and focus of the current development of the oil industry, with huge potential economic value and social benefits. Therefore, it is very necessary to develop a high-strength and high-corrosion-resistant super martensitic stainless steel, so that it can be widely used in the field of oil and gas engineering. Summary of the invention

[0004] In view of the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a high-strength and high-corrosion-resistant super martensitic stainless steel, a preparation method and application thereof.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The first aspect of the present invention provides a high-strength and high-corrosion-resistant super martensitic stainless steel, which comprises the following element components by mass percentage: C 0.02-0.04%, Cr 12-18%, Mo 0.5-2%, Ni 4-8%, Cu 0.5-1.5%, P≤0.02%, S≤0.02% and the balance is Fe.

[0007] Preferably, the alloy comprises the following element components by mass percentage: C 0.02%, Cr 14%, Mo 1%, Ni 5%, Cu 1%, P≤0.02%, S≤0.02% and the balance is Fe.

[0008] Preferably, the alloy comprises the following element components by mass percentage: C 0.02%, Cr 18%, Mo 0.5%, Ni 8%, Cu 1.5%, P≤0.02%, S≤0.02% and the balance is Fe.

[0009] Preferably, the alloy comprises the following element components by mass percentage: C 0.04%, Cr 12%, Mo 2%, Ni 6%, Cu 0.5%, P≤0.02%, S≤0.02% and the balance is Fe.

[0010] The selection and addition of alloying elements for the high-strength and high-corrosion-resistant super martensitic stainless steel prepared by the present invention follow the following principles: ensuring that the stainless steel is a full martensitic or nearly full martensitic structure, ensuring the cleanliness and corrosion resistance of the steel, improving the hardenability of the stainless steel, improving the yield strength and tensile strength of the stainless steel, while ensuring that the stainless steel still has good elongation, and reducing raw material costs and production costs.

[0011] The second object of the present invention is to provide a method for preparing the above-mentioned high-strength and high-corrosion-resistant super martensitic stainless steel, comprising the following steps:

[0012] S1. Weigh the raw materials according to the formula, melt them, and cast them to obtain steel billets;

[0013] S2, subjecting the obtained steel billet to a first homogenization treatment and heat preservation to obtain a square billet;

[0014] S3, forging the obtained square billet, cooling it, and obtaining a crude stainless steel product;

[0015] S4. The obtained stainless steel crude product is subjected to a second homogenization treatment, heat preservation, and cooling to obtain super martensitic stainless steel.

[0016] Preferably, in step S2, the temperature of the first homogenization treatment is 1050-1250°C, for example, it can be 1050°C, 1100°C, 1150°C, 1200°C, 1250°C; the treatment time is 0.5-3h, for example, it can be 0.5h, 1h, 2h, 3h.

[0017] Preferably, in step S3, the forging process includes: two stages of preliminary forging and final forging, the temperature of the initial forging is 1150-1250°C, for example, it can be 1150°C, 1200°C, 1250°C; the temperature of the final forging is 950-1050°C, for example, it can be 950°C, 1000°C, 1025°C, 1050°C; the forging ratio is greater than 7.

[0018] Preferably, in step S4, the temperature of the second homogenization treatment is 1050-1250°C, for example, it can be 1050°C, 1100°C, 1150°C, 1200°C, 1250°C; the insulation time is 0.5-3h, for example, it can be 0.5h, 1h, 2h, 3h; the cooling method is water cooling to room temperature.

[0019] A third object of the present invention is to provide application of the above-mentioned super martensitic stainless steel in marine engineering.

[0020] The present invention has the following beneficial effects:

[0021] The invention prepares a super martensitic stainless steel by reasonably selecting and controlling alloy elements and their contents, and the super martensitic stainless steel has a lower content of Ni element, higher yield strength and tensile strength and good electrochemical corrosion resistance.

[0022] The preparation method of the present invention does not require secondary tempering, has a simple process, a stable and convenient process, and a low raw material cost, is suitable for industrial production, and is applied in the field of marine engineering to further reduce the cost of steel materials for marine engineering, and is expected to replace the application of 316L stainless steel in the field of marine engineering. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 The microstructure of the high-strength and high-corrosion-resistant super martensitic stainless steel obtained in Example 1;

[0025] Figure 2 The grain orientation of the high-strength and high-corrosion-resistant super martensitic stainless steel obtained in Example 1;

[0026] Figure 3 The microstructure of the high-strength and high-corrosion-resistant super martensitic stainless steel obtained in Example 2;

[0027] Figure 4The microstructure of the high-strength and high-corrosion-resistant super martensitic stainless steel obtained in Example 3;

[0028] Figure 5 The microstructure of the high-strength and high-corrosion-resistant super martensitic stainless steel obtained in Example 4;

[0029] Figure 6 The microstructure of the high-strength and high-corrosion-resistant super martensitic stainless steel obtained in Example 5;

[0030] Figure 7 This is the microstructure of the high-strength and high-corrosion-resistant super martensitic stainless steel obtained in Example 6. DETAILED DESCRIPTION

[0031] In the following description, for the purpose of illustration rather than limitation, specific details such as specific system structures and technologies are provided to provide a thorough understanding of the embodiments of the present invention. However, it should be clear to those skilled in the art that the present invention may also be implemented in other embodiments without these specific details.

[0032] Example 1

[0033] A high-strength and high-corrosion-resistant super martensitic stainless steel, comprising the following element components by mass percentage: C 0.02%, Cr 14%, Mo 1%, Ni 5%, Cu 1%, P ≤ 0.02%, S ≤ 0.02% and the balance is Fe. The preparation method thereof comprises the following steps:

[0034] S1, weighing the raw materials according to the above-mentioned component ratio and smelting, and pouring the molten steel to obtain a steel billet;

[0035] S2, placing the obtained cast steel billet at 1150° C. for a first homogenization treatment, keeping the temperature for 2 hours, to obtain a stainless steel billet;

[0036] S3, forging the obtained stainless steel billet, with an initial forging temperature of 1200° C., a final forging temperature of 1000° C., a forging ratio greater than 7, and then water cooling to room temperature to obtain a stainless steel square billet;

[0037] S4. The obtained stainless steel square billet is subjected to a second homogenization treatment at 1150° C., kept at this temperature for 2 hours, and water-cooled to room temperature to obtain super martensitic stainless steel.

[0038] The obtained super martensitic stainless steel was subjected to wire cutting sampling, rough grinding, fine grinding, polishing, deionized water ultrasonic cleaning and drying treatment. The microstructure and grain orientation were observed by scanning electron microscopy. Figure 1 and Figure 2 The yield strength, tensile strength, corrosion potential and corrosion current were measured using a universal testing machine and an electrochemical workstation. The results are shown in Table 1.

[0039] Depend on Figure 1 The results show that the super martensitic stainless steel obtained in Example 1 is a full martensitic phase structure, does not contain other phases such as ferrite or austenite, and has a uniform composition without segregation. Figure 2 The results show that the super martensitic stainless steel obtained in Example 1 has a random orientation distribution, does not have a specific grain orientation, and does not cause obvious anisotropy in the mechanical properties of the material.

[0040] Example 2

[0041] A high-strength and high-corrosion-resistant super martensitic stainless steel, comprising the following element components by mass percentage: C 0.02%, Cr 18%, Mo 0.5%, Ni 8%, Cu 1.5%, P ≤ 0.02%, S ≤ 0.02% and the balance Fe. The preparation method thereof comprises the following steps:

[0042] S1, weighing the raw materials according to the above-mentioned component ratio and smelting, and pouring the molten steel to obtain a steel billet;

[0043] S2, placing the obtained cast steel billet at 1050° C. for a first homogenization treatment, keeping the temperature for 3 hours, to obtain a stainless steel billet;

[0044] S3, forging the obtained stainless steel billet, with an initial forging temperature of 1150° C., a final forging temperature of 950° C., a forging ratio greater than 7, and then water cooling to room temperature to obtain a stainless steel square billet;

[0045] S4. The obtained stainless steel square billet is subjected to a second homogenization treatment at 1050° C., kept at this temperature for 3 hours, and water-cooled to room temperature to obtain super martensitic stainless steel.

[0046] The obtained super martensitic stainless steel was subjected to wire cutting sampling, rough grinding, fine grinding, polishing, deionized water ultrasonic cleaning and drying treatment. The microstructure was observed by scanning electron microscopy. Figure 3 The yield strength, tensile strength, corrosion potential and corrosion current were measured using a universal testing machine and an electrochemical workstation. The results are shown in Table 1.

[0047] Depend on Figure 3 The results show that the super martensitic stainless steel obtained in Example 2 has a full martensitic phase structure, does not contain other phases such as ferrite or austenite, and has a uniform composition without segregation.

[0048] Example 3

[0049] A high-strength and high-corrosion-resistant super martensitic stainless steel, comprising the following element components by mass percentage: C0.04%, Cr 12%, Mo 2%, Ni 6%, Cu 0.5%, P≤0.02%, S≤0.02% and the balance is Fe. The preparation method thereof comprises the following steps:

[0050] S1, weighing the raw materials according to the above-mentioned component ratio and smelting, and pouring the molten steel to obtain a steel billet;

[0051] S2, placing the obtained cast steel billet at 1250° C. for a first homogenization treatment, keeping the temperature for 0.5 h, to obtain a stainless steel billet;

[0052] S3, forging the obtained stainless steel billet, with an initial forging temperature of 1250° C., a final forging temperature of 1050° C., a forging ratio greater than 7, and then water cooling to room temperature to obtain a stainless steel square billet;

[0053] S4. The obtained stainless steel square billet is subjected to a second homogenization treatment at 1250° C., kept at this temperature for 0.5 h, and water-cooled to room temperature to obtain super martensitic stainless steel.

[0054] The super martensitic stainless steel obtained in Example 3 was subjected to wire cutting sampling, rough grinding, fine grinding, polishing, ultrasonic cleaning with deionized water and drying treatment. The microstructure was observed by scanning electron microscopy. Figure 4 The yield strength, tensile strength, corrosion potential and corrosion current were measured using a universal testing machine and an electrochemical workstation. The results are shown in Table 1.

[0055] Depend on Figure 4 The results show that the super martensitic stainless steel obtained in Example 3 has a full martensitic phase structure, does not contain other phases such as ferrite or austenite, and has a uniform composition without segregation.

[0056] Example 4

[0057] A high-strength and high-corrosion-resistant super martensitic stainless steel, comprising the following element components by mass percentage: C 0.02%, Cr 18%, Mo 1%, Ni 5%, Cu 1%, P≤0.02%, S≤0.02% and the balance is Fe. The preparation method thereof comprises the following steps:

[0058] S1, weighing the raw materials according to the above-mentioned component ratio and smelting, and pouring the molten steel to obtain a steel billet;

[0059] S2, placing the obtained cast steel billet at 1150° C. for a first homogenization treatment, keeping the temperature for 2 hours, to obtain a stainless steel billet;

[0060] S3, forging the obtained stainless steel billet, with an initial forging temperature of 1250° C., a final forging temperature of 1000° C., a forging ratio greater than 7, and then water cooling to room temperature to obtain a stainless steel square billet;

[0061] S4. The obtained stainless steel square billet is subjected to a second homogenization treatment at 1150° C., kept at this temperature for 2 hours, and water-cooled to room temperature to obtain super martensitic stainless steel.

[0062] The super martensitic stainless steel obtained in Example 4 was subjected to wire cutting sampling, rough grinding, fine grinding, polishing, ultrasonic cleaning with deionized water and drying treatment. The microstructure was observed by scanning electron microscopy. Figure 5 The yield strength, tensile strength, corrosion potential and corrosion current were measured using a universal testing machine and an electrochemical workstation. The results are shown in Table 1.

[0063] Depend on Figure 5 The results show that the super martensitic stainless steel obtained in Example 4 has a full martensitic phase structure, does not contain other phases such as ferrite or austenite, and has a uniform composition without segregation.

[0064] Example 5

[0065] A high-strength and high-corrosion-resistant super martensitic stainless steel, comprising the following element components by mass percentage: C 0.02%, Cr 16%, Mo 1%, Ni 7%, Cu 1.5%, P ≤ 0.02%, S ≤ 0.02% and the balance is Fe. The preparation method thereof comprises the following steps:

[0066] S1, weighing the raw materials according to the above-mentioned component ratio and smelting, and pouring the molten steel to obtain a steel billet;

[0067] S2, placing the obtained cast steel billet at 1200° C. for a first homogenization treatment, keeping the temperature for 1.5 hours, to obtain a stainless steel billet;

[0068] S3, forging the obtained stainless steel billet, with an initial forging temperature of 1200° C., a final forging temperature of 1050° C., a forging ratio greater than 7, and then water cooling to room temperature to obtain a stainless steel square billet;

[0069] S4. The obtained stainless steel square billet is subjected to a second homogenization treatment at 1200° C., kept at this temperature for 1.5 hours, and water-cooled to room temperature to obtain super martensitic stainless steel.

[0070] The super martensitic stainless steel obtained in Example 5 was subjected to wire cutting sampling, rough grinding, fine grinding, polishing, ultrasonic cleaning with deionized water and drying treatment. The microstructure was observed by scanning electron microscopy. Figure 6 The yield strength, tensile strength, corrosion potential and corrosion current were measured using a universal testing machine and an electrochemical workstation. The results are shown in Table 1.

[0071] Depend on Figure 6 The results show that the obtained super martensitic stainless steel has a full martensitic phase structure, does not contain other phases such as ferrite or austenite, and has a uniform composition without segregation.

[0072] Example 6

[0073] A high-strength and high-corrosion-resistant super martensitic stainless steel, comprising the following element components by mass percentage: C 0.02%, Cr 13%, Mo 1%, Ni 5%, Cu 1.5%, P ≤ 0.02%, S ≤ 0.02% and the balance is Fe. The preparation method thereof comprises the following steps:

[0074] S1, weighing the raw materials according to the above-mentioned component ratio and smelting, and pouring the molten steel to obtain a steel billet;

[0075] S2, placing the obtained cast steel billet at 1150° C. for a first homogenization treatment, keeping the temperature for 2 hours, to obtain a stainless steel billet;

[0076] S3, forging the obtained stainless steel billet, with an initial forging temperature of 1150° C., a final forging temperature of 1000° C., a forging ratio greater than 7, and then water cooling to room temperature to obtain a stainless steel square billet;

[0077] S4. The obtained stainless steel square billet is subjected to a second homogenization treatment at 1150° C., kept at this temperature for 2 hours, and water-cooled to room temperature to obtain super martensitic stainless steel.

[0078] The super martensitic stainless steel obtained in Example 6 was subjected to wire cutting sampling, rough grinding, fine grinding, polishing, ultrasonic cleaning with deionized water and drying treatment. The microstructure was observed by scanning electron microscopy. Figure 7 The yield strength, tensile strength, corrosion potential and corrosion current were measured using a universal testing machine and an electrochemical workstation. The results are shown in Table 1.

[0079] Depend on Figure 7 The results show that the obtained super martensitic stainless steel has a full martensitic phase structure, does not contain other phases such as ferrite or austenite, and has a uniform composition without segregation.

[0080] Comparative Example 1

[0081] The method is basically the same as Example 1, except that no Ni is added, thereby obtaining Ni-free martensitic stainless steel.

[0082] The Ni-free martensitic stainless steel obtained in Comparative Example 1 was subjected to experimental tests on yield strength, tensile strength, corrosion potential and corrosion current using a universal testing machine and an electrochemical workstation. The results are shown in Table 1.

[0083] Comparative Example 2

[0084] The method is basically the same as Example 1, except that no Cu is added to obtain Cu-free super martensitic stainless steel.

[0085] The yield strength, tensile strength, corrosion potential and corrosion current of the Cu-free super martensitic stainless steel obtained in Comparative Example 2 were tested using a universal testing machine and an electrochemical workstation. The results are shown in Table 1.

[0086] Comparative Example 3

[0087] The method is basically the same as Example 1, except that 5% Cu is added to obtain super martensitic stainless steel with high Cu content.

[0088] The yield strength, tensile strength, corrosion potential and corrosion current of the high Cu content super martensitic stainless steel obtained in Comparative Example 3 were tested using a universal testing machine and an electrochemical workstation. The results are shown in Table 1.

[0089] Comparative Example 4

[0090] The method is basically the same as Example 1, except that in step S3, the initial forging temperature is 950° C. and the final forging temperature is 800° C. Thus, forged super martensitic stainless steel is obtained.

[0091] The yield strength, tensile strength, corrosion potential and corrosion current of the low temperature forged super martensitic stainless steel obtained in Comparative Example 4 were tested using a universal testing machine and an electrochemical workstation. The results are shown in Table 1.

[0092] Comparative Example 5

[0093] The method is basically the same as Example 1, except that in step S3, the initial forging temperature is 1250° C. and the final forging temperature is 1150° C. Thus, forged super martensitic stainless steel is obtained.

[0094] The yield strength, tensile strength, corrosion potential and corrosion current of the high temperature forged super martensitic stainless steel obtained in Comparative Example 5 were tested using a universal testing machine and an electrochemical workstation. The results are shown in Table 1.

[0095] Table 1. Mechanical properties and electrochemical corrosion performance test results

[0096]

[0097]

[0098] From the results in Table 1, it can be seen that the yield strength of the Ni-free super martensitic stainless steel prepared in Comparative Example 1 is 880±13MPa, the tensile strength is 1030±7MPa, the elongation is 10±5%, the corrosion potential is -0.3801±0.030V, and the corrosion current is 4.0±0.1×10 -11 Am 2 The comprehensive performance is significantly lower than that of the super martensitic stainless steel obtained in Examples 1-6. The stainless steel contains a certain amount of ferrite phase, which results in that its strength is not significantly improved but its elongation is greatly reduced. The yield strength of the Cu-free super martensitic stainless steel obtained in Comparative Example 2 is 920±15MPa, the tensile strength is 1039±8MPa, the elongation is 17±2%, the corrosion potential is -0.3776±0.030V, and the corrosion current is 3.7±0.1×10 -11 Am 2 The comprehensive performance is significantly lower than that of the super martensitic stainless steel obtained in Examples 1-6. This is because the addition of a certain amount of Cu can improve the plasticity of the super martensitic stainless steel and improve the corrosion resistance of the material. The super martensitic stainless steel obtained in Comparative Example 3 has a brittle fracture when its strength reaches about 720 MPa, a yield strength of 720 ± 15 MPa, and an undetected tensile strength. The elongation is less than 1%, the corrosion potential is -0.3501 ± 0.050 V, and the corrosion current is 3.5 ± 0.1 × 10 -11 Am 2 . The mechanical properties of the high Cu content super martensitic stainless steel are lower than those of the super martensitic stainless steel of Examples 1-6, and the stainless steel contains a certain amount of Cu-containing compound phase. This is because the high Cu content super martensitic stainless steel is prone to segregate finely dispersed Cu compound phases containing elements such as Fe, Cr and Ni, thereby changing the distribution of martensitic Fe, Cr and Ni components in the stainless steel, greatly reducing the elastic plasticity of the material and easily causing crack sources and brittle fracture. In addition, the Cu element in the high Cu content super martensitic stainless steel is prone to form brittle compounds such as Cu2O and Cu2S with O and S elements during the preparation process. The yield strength of the forged super martensitic stainless steel obtained in Comparative Example 4 is 828±20MPa, the tensile strength is 958±10MPa, the elongation is 13±2%, the corrosion potential is -0.3440±0.010V, and the corrosion current is 3.1±0.1×10 -11 Am 2The mechanical properties of the forged super martensitic stainless steel prepared at this relatively low temperature are significantly lower than those of Example 1, because the forging temperature is too low to refine the core grain structure of the material. The yield strength of the forged super martensitic stainless steel prepared at a higher temperature in Comparative Example 5 is 789±30MPa, the tensile strength is 926±30MPa, the elongation is 10±3%, the corrosion potential is -0.3433±0.010V, and the corrosion current is 3.1±0.1×10 -11 Am 2 The mechanical properties of the super martensitic stainless steel forged at this relatively high temperature are significantly lower than those of Example 1. This is because the excessively high forging temperature causes the grains of the material to grow.

[0099] The super martensitic stainless steel prepared in Examples 1 to 6 of the present invention has higher yield strength, tensile strength and better electrochemical corrosion resistance, and its comprehensive performance exceeds that of commercial 00Cr13Ni5Mo super martensitic stainless steel and 316 stainless steel. As a high-performance metal material, it has broad application prospects in marine engineering.

[0100] The present invention is not limited to the above-mentioned specific implementation modes. Various changes made by ordinary technicians in this field based on the above-mentioned concepts without creative work are all within the protection scope of the present invention.

Claims

1. A high-strength and high-corrosion-resistant super martensitic stainless steel, characterized in that: The invention comprises the following element components by mass percentage: C 0.02-0.04%, Cr 12-18%, Mo 0.5-2%, Ni 4-8%, Cu 0.5-1.5%, P≤0.02%, S≤0.02% and the balance is Fe.

2. The high-strength and high-corrosion-resistant super martensitic stainless steel according to claim 1, characterized in that: The alloy comprises the following elements in percentage by mass: C 0.02%, Cr 14%, Mo 1%, Ni 5%, Cu 1%, P≤0.02%, S≤0.02% and the balance is Fe.

3. The high-strength and high-corrosion-resistant super martensitic stainless steel according to claim 1, characterized in that: The alloy comprises the following elements in percentage by mass: C 0.02%, Cr 18%, Mo 0.5%, Ni 8%, Cu 1.5%, P≤0.02%, S≤0.02% and the balance is Fe.

4. The high-strength and high-corrosion-resistant super martensitic stainless steel according to claim 1, characterized in that: The alloy comprises the following elements in percentage by mass: C 0.04%, Cr 12%, Mo 2%, Ni 6%, Cu 0.5%, P≤0.02%, S≤0.02% and the balance is Fe.

5. A method for preparing the high-strength and high-corrosion-resistant super martensitic stainless steel according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Weigh the raw materials according to the formula, melt them, and cast them to obtain steel billets; S2, subjecting the obtained steel billet to a first homogenization treatment and heat preservation to obtain a square billet; S3, forging the obtained square billet, cooling it, and obtaining a crude stainless steel product; S4. The obtained stainless steel crude product is subjected to a second homogenization treatment, heat preservation, and cooling to obtain super martensitic stainless steel.

6. The method for preparing high-strength and high-corrosion-resistant super martensitic stainless steel according to claim 5, characterized in that: In step S2, the temperature of the first homogenization treatment is 1050-1250°C, and the treatment time is 0.5-3h.

7. The method for preparing high-strength and high-corrosion-resistant super martensitic stainless steel according to claim 5, characterized in that: In step S3, the forging process includes two stages: initial forging and final forging. The temperature of the initial forging is 1150-1250°C, the temperature of the final forging is 950-1050°C, and the forging ratio is greater than 7.

8. The method for preparing high-strength and high-corrosion-resistant super martensitic stainless steel according to claim 5, characterized in that: In step S4, the temperature of the second homogenization treatment is 1050-1250° C., and the holding time is 0.5-3 h.

9. The method for preparing high-strength and high-corrosion-resistant super martensitic stainless steel according to claim 5, characterized in that: In step S4, the cooling method is water cooling to room temperature.

10. Application of the high-strength and high-corrosion-resistant super martensitic stainless steel according to claim 1 in marine engineering.

Citation Information

Patent Citations

  • Cl<-> point corrosion resistant super martensitic stainless steel and heat treatment method thereof

    CN102703829A

  • Molybdenum-copper composite reinforced martensitic stainless steel and preparation method thereof

    CN117867394A

  • Production of martensitic stainless steel excellent in co2 corrosion resistance and sulfide stress cracking resistance

    JP1996260038A

  • Production of martensitic stainless steel excellent in co2 corrosion resistance and sulfide stress cracking resistance

    JP1996260041A