Heat treatment method for hub

Through low-temperature solid solution heat treatment and aging process optimization, the deformation and surface oxidation of aluminum alloy wheel hubs are solved, the mechanical properties and elongation are improved, the requirements of new energy vehicles for wheel performance and quality are met, and energy consumption is reduced.

CN119020707APending Publication Date: 2024-11-26ZHEJIANG WANFENG LIGHT ALLOY RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411143223.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing high-temperature solution heat treatment process leads to deformation, surface oxidation and high energy consumption of aluminum alloy wheel hubs, which cannot meet the higher requirements of new energy vehicles for wheel performance and quality.

Method used

The chemical composition and aging process of A356.2 alloy are optimized by using low-temperature solution heat treatment method, including low-temperature solution at 480-530℃, water quenching at 20-90℃ and aging treatment at 150-180℃ to reduce heat treatment deformation. Improve elongation and reduce energy consumption.

Benefits of technology

It effectively solves the problems of heat treatment deformation and surface quality of the wheel hub, improves mechanical properties and elongation, and reduces energy consumption and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a heat treatment method for a hub, which is characterized by comprising the following steps: placing the hub to be treated in heat treatment equipment for low-temperature solid solution heat treatment, and preserving heat for a first time in a first temperature range in the low-temperature solid solution heat treatment; the hub subjected to solid solution heat treatment is placed in water to be quenched, quenching is carried out in water, quenching is kept within a second temperature range for second time, and the hub is taken out after quenching is carried out; and the hub is subjected to aging treatment, the aging treatment is carried out within a third temperature range, and the aging treatment is kept for a third time. According to the method, through low-temperature solid solution, deformation after heat treatment quenching can be remarkably reduced while the mechanical property is kept unchanged or even improved, the alloy can better meet the characteristics of a low-temperature solid solution heat treatment process, and the mechanical property of an existing hub is kept or improved while deformation is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of heat treatment and material alloying, and more specifically, relates to a low-temperature solid solution heat treatment method for an aluminum alloy wheel hub. Background Art

[0002] Aluminum alloy wheels have become the mainstream choice of automobile wheel materials due to their light weight, high strength and good thermal conductivity, especially with the application of low-pressure casting technology, and their market share is as high as about 80%. At present, low-pressure cast aluminum alloy wheels on the market generally use A356.2 alloy, which is widely used due to its excellent comprehensive performance. In order to ensure the mechanical properties of aluminum alloy wheels, high-temperature heat treatment processes are generally used in the industry. The process includes two stages: solution treatment and artificial aging. Solution treatment is usually carried out in the temperature range of 535-545℃, aiming to completely dissolve the Mg2Si phase formed in the cast state into the a-Al matrix. The subsequent artificial aging treatment is carried out at a temperature of 130-155℃, which promotes the precipitation of fine and dispersed Mg2Si phases, thereby strengthening the material.

[0003] However, the existing high-temperature solution treatment process has several problems. First, the high-temperature solution is close to the solidus line of the material, which leads to severe softening of the material, increasing the risk of thermal stress during quenching, which in turn causes wheel deformation and causes a large number of products to be scrapped. This problem is particularly prominent against the backdrop of the rise of new energy vehicles, because new energy vehicles are usually heavier, require larger wheels, and have more complex shapes. The wheel deformation problem is more serious, becoming a pain point for wheel manufacturers.

[0004] Secondly, high temperature solution treatment will also cause serious oxidation on the wheel surface, resulting in blackening of the surface, which affects the surface quality of the wheel. For wheels with higher surface quality requirements, additional grinding steps are required to remove the oxide layer, which not only increases production costs, but also prolongs the production cycle.

[0005] In addition, high-temperature solution treatment will also lead to a large consumption of energy, which is not conducive to sustainable development and environmental protection.

[0006] Although the industry has explored the low-temperature solution process, due to the mismatch between chemical composition and aging process, the mechanical properties of products after low-temperature solution treatment often cannot meet the requirements of industrial applications, resulting in the entire industry still generally using high-temperature solution treatment.

[0007] In view of the above problems, the present invention aims to provide an improved low-temperature solution heat treatment of aluminum alloy wheels and its alloy optimization process to solve the defects in the prior art, improve the mechanical properties of the wheels, reduce energy consumption and product scrap rate in the production process, and meet the higher requirements of new energy vehicles for wheel performance and quality. Summary of the invention

[0008] The purpose of the present invention is to provide a heat treatment method for a wheel hub, which optimizes the chemical composition and aging process of the A356.2 alloy accordingly, while greatly reducing the heat treatment deformation, maintaining the same mechanical performance indicators, and at the same time the elongation can be improved.

[0009] To achieve the above object, the technical solution adopted by the present invention includes:

[0010] A heat treatment method for a wheel hub comprises the following steps:

[0011] The wheel hub to be treated is placed in a heat treatment device for low-temperature solution heat treatment, and the low-temperature solution heat treatment is kept within a first temperature range for a first time; the wheel hub after the solution heat treatment is placed in water for quenching, and the quenching is carried out in water, and the quenching is kept within a second temperature range for a second time, and the wheel hub is taken out after the quenching; the wheel hub is subjected to aging treatment, and the aging treatment is carried out within a third temperature range and kept for a third time.

[0012] Optionally, after the low-temperature solution heat treatment, the hub is placed in water within 25 seconds.

[0013] Optionally, the first temperature range is 480-530° C., and the first time is 4-12 hours.

[0014] Optionally, the second temperature range is 20-90° C., and the second time is 15-30 minutes.

[0015] Optionally, the third temperature range is 150-180° C., and the third time is 2-8 hours.

[0016] Optionally, the wheel hub to be processed is made of low-pressure cast aluminum alloy, and the low-pressure cast aluminum alloy comprises, in terms of chemical composition mass percentage:

[0017] Si 6.6-7.4%; Fe<0.15%; Mg 0.20-0.30%; Cu 0.20-0.40%; Sr0.008-0.02%; Ti 0.08-0.3%; Mn<0.10%; Ni, Zn<0.02%; Pb, Sn<0.01%; Zr<0.01%; Ca<0.003%.

[0018] Optionally, the wheel hub to be processed is prepared by the following steps: a. adding alloy ingots and recycled materials into a melting furnace for smelting, deslagging in the furnace within a temperature range of 760-800°C to form molten metal, and pouring the molten metal into a transfer bag; b. adding Mg, Ti, and Sr elements to the transfer bag to adjust the chemical composition, and then degassing and deslagging in the transfer bag; c. pouring the molten metal into a low-pressure casting insulation furnace to perform low-pressure casting of a wheel hub blank, and deburring and pouring riser treatment on the wheel hub blank to obtain the wheel hub to be processed.

[0019] Optionally, the Ti element is added to the transfer bag in the form of an Al-5%-Ti-1% master alloy, Mg is added in the form of pure Mg or an Al-Mg master alloy, and Sr is added in the form of Al-10%Sr.

[0020] Optionally, the method further includes, after the molten metal in the transfer ladle is degassed and deslagging is carried out, performing a vacuum density test on the molten metal, the test being carried out at 720-760°C to ensure that the vacuum density test requirement is 2.65g / cm3.

[0021] Optionally, during the low-pressure casting of the wheel hub blank, a filter screen is added to the liquid inlet at the bottom of the mold, and the filter screen is only used for the low-pressure casting of one wheel hub blank.

[0022] The present invention provides an optimized A356.2 low-pressure casting aluminum alloy, which mainly reduces the Mg content and adds a small amount of Cu. The lower Mg content is mainly to adapt to the low-temperature solid solution process. Under the low-temperature solid solution state, it can also ensure that all Mg in Mg2Si can be dissolved in the a-Al matrix to achieve the effect of solid solution. The addition of Cu mainly plays a role in solid solution strengthening, compensating for the strengthening effect caused by the reduction of Mg.

[0023] The present invention also provides a new aging heat treatment process, with an aging temperature of 150-180°C and a heat preservation time of 2-8 hours. In order to ensure the elongation, the cast aluminum wheel hub generally adopts a lower aging temperature of 130-150°C. The present invention increases the aging temperature to 150-180°C to increase the strengthening effect, so that less Mg2Si strengthening phase can achieve a greater effect. At the same time, due to the reduction of Mg, the elongation can still be maintained at a high level even under high temperature aging.

[0024] The beneficial effect of the present invention is that compared with the prior art, the present invention solves the deformation problem of the wheel hub after heat treatment through a low-temperature solid solution heat treatment process. At the same time, through the optimization of chemical composition and aging process, while ensuring the strength of the material, the elongation can also be improved. At the same time, the present invention also solves the problem of heat treatment deformation of the aluminum wheel hub. Due to the reduction of the solid solution temperature, the wheel hub also has a good surface quality, the blackening of the surface due to heat treatment is reduced, and the sandblasting operation is reduced. The reduction of the solid solution temperature also reduces energy consumption and the damage to the furnace group caused by high-temperature solid solution. DETAILED DESCRIPTION

[0025] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in combination with specific descriptions and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] First, the present invention provides a heat treatment method for a wheel hub, the method comprising the following steps:

[0027] Placing the wheel hub to be treated in a heat treatment device for low-temperature solid solution heat treatment, wherein the low-temperature solid solution heat treatment is maintained within a first temperature range for a first time;

[0028] Placing the wheel hub after the solution heat treatment into water for quenching, wherein the quenching is performed in water, the quenching is maintained within a second temperature range for a second time, and the wheel hub is taken out after the quenching;

[0029] The hub is subjected to an aging treatment, wherein the aging treatment is performed within a third temperature range and the aging treatment is maintained for a third time.

[0030] In order to ensure that the wheel hub can be quickly immersed in water after solution heat treatment, the wheel hub and the heat treatment rack are immersed in water at the same time, which can also facilitate the removal of the wheel hub from the water. Of course, the wheel hub can also be placed in water alone, but it must be ensured that the wheel hub is immersed in water within 25 seconds. The initial temperature of the water is controlled at 20-90℃, and the wheel hub is taken out of the water after being immersed in water for 15 minutes.

[0031] In a preferred embodiment, the first temperature range is 480-530°C, and the first time is 4-12 hours. Preferably, the temperature of the solution heat treatment is 510°C, and the holding time is 8 hours.

[0032] The second temperature range is 20-90° C., and the second time is 15-30 minutes.

[0033] The third temperature range is 150-180°C, and the third time is 2-8 hours. After the hub is drained, preferably, the aging treatment temperature is 170°C and the time is 4 hours. In order to make the hub achieve the required mechanical properties, the aging temperature and time are interrelated. A lower aging temperature uses a longer aging time, and a higher aging temperature uses a shorter aging time.

[0034] The deformation problem of the wheel hub after heat treatment is solved by the low-temperature solution heat treatment process. At the same time, by optimizing the chemical composition and aging process, the elongation can be improved while ensuring the material strength. At the same time, the invention also solves the problem of heat treatment deformation of the aluminum wheel hub. Due to the reduction of the solution temperature, the wheel hub also has good surface quality, the blackening of the surface during heat treatment is reduced, and the sandblasting operation is reduced. The reduction of the solution temperature also reduces energy consumption and the damage to the furnace group caused by high-temperature solution.

[0035] In order to achieve low temperature solid solution, the proportion of the aluminum alloy itself as the target of low temperature solid solution is also very important. Now, a low pressure casting aluminum alloy optimized based on A356.2 alloy provided by the present invention is described. Among them, the wheel hub to be processed is made of low pressure casting aluminum alloy, and the low pressure casting aluminum alloy includes, in terms of chemical composition mass percentage:

[0036] Si 6.6-7.4%; Fe<0.15%; Mg 0.20-0.30%; Cu 0.20-0.40%; Sr0.008-0.02%; Ti 0.08-0.3%; Mn<0.10%; Ni, Zn<0.02%; Pb, Sn<0.01%; Zr<0.01%; Ca<0.003%.

[0037] In the design of optimizing the chemical composition of the alloy, the Mg content in the A356.2 alloy was reduced and a small amount of Cu was added. The reduction in Mg content reduces the number of Mg2Si precipitation strengthening phases during the aging process, which correspondingly reduces the strengthening effect. However, the addition of Cu plays a role in solid solution strengthening, compensating for the effect of Mg reduction. Since a small amount of Cu is added to only strengthen the a-Al solid solution and does not produce precipitation strengthening, it has a high elongation while maintaining strength. Therefore, through the joint optimization of low-temperature solid solution, chemical composition and aging process, it can not only reduce heat treatment deformation, but also maintain strength and improve elongation.

[0038] In a preferred embodiment, the preparation of low pressure casting aluminum alloy comprises the following steps:

[0039] a. Add alloy ingots and recycled materials into the furnace for smelting, remove the slag in the furnace, and pour the molten metal into the transfer bag after reaching the preset temperature.

[0040] The added amounts of alloy ingots and recycled materials are proportioned according to the requirements of the chemical composition of the wheel hub. When removing slag in the furnace, it is necessary to do it at least three times. Each time the slag on the surface of the molten metal is scraped off, the slag should be scraped off in different directions at least three times until the surface of the molten metal is completely bright and there is no floating slag.

[0041] Preferably, the preset temperature of the molten metal is 760-800°C.

[0042] b. The final chemical composition is adjusted in the transfer bag, mainly by adding Mg, Sr and Ti. Mg is mainly used to improve the strength of the alloy. Sr is added to quench and temper the eutectic Si and change the morphology of the eutectic Si. By adding Ti, the aluminum alloy is refined to improve the flow properties of the alloy and reduce micro-shrinkage.

[0043] In the process of adding Mg element, it can be added in the form of pure Mg or in the form of Al-Mg master alloy; Sr is added in the form of Al-10%Sr master alloy; similarly, Ti is added in the form of Al-Al-5%Ti-1%B master alloy, and degassing treatment can be carried out only after addition, so as to achieve full dissolution and mixing of Mg, Sr and Ti elements in the molten metal.

[0044] After adding various alloy elements, it is necessary to add a special aluminum alloy slag remover for slag removal. Sprinkle about 0.1% of the weight of the solution on the surface of the molten metal, and then degasify. The degassing treatment is carried out by passing nitrogen into a rotary degasser. After the degassing is completed, let it stand for about 10 minutes. Degassing and slag removal can not only effectively discharge hydrogen in the molten metal, but also remove other harmful substances such as oxidized slag, etc.

[0045] After the metal liquid in the transfer bag is degassed and deslagging, the density of the metal liquid is tested. The vacuum density value is required to be 2.65g / cm 3 ,The temperature of the molten metal after degassing in the transfer bag is 720-760℃.

[0046] c. Pour the molten metal into a low-pressure casting insulation furnace to prepare a wheel hub blank, and perform burr removal and pouring riser treatment on the wheel hub blank.

[0047] When casting the wheel hub blank at low pressure, add a filter screen to the liquid inlet at the bottom of the mold, and one filter screen is required for each mold. After the wheel hub blank is taken out of the mold, the pouring head is removed by sawing, and the burrs are removed by grinding after sawing.

[0048] d. Perform the above-mentioned aluminum alloy wheel low temperature solid solution + optimized aging heat treatment process on the wheel hub blank to make the wheel hub meet the mechanical performance requirements;

[0049] e. Rough turning, painting and finish turning are performed on the wheel hub in sequence.

[0050] After rough turning, the wheel hub is spray-painted and the heating process of the painting process is carried out according to the process approved by the workshop.

[0051] The present invention uses a low-temperature solid solution heat treatment process and optimizes the chemical composition and aging process, which not only greatly reduces the deformation of the wheel hub during heat treatment, but also has a higher elongation while maintaining the strength of the wheel hub, perfectly solving the pain points in the wheel hub industry.

[0052] Example:

[0053] After alloy melting, degassing, standing, and chemical composition adjustment, two groups of alloys with the following composition are cast. The first group is the standard A356.2 alloy, and the second group is an optimized alloy with reduced Mg content and a small amount of Cu added, please refer to Table 1:

[0054] Table 1

[0055]

[0056] After the two alloys were cast and formed, the wheels were sawn and poured, and then heat treated by four heat treatment processes, namely 540℃X6h+130℃X3h (original heat treatment process), 540℃X6h+170℃X3h, 520℃X6h+130℃X3h, 520℃X6h+170℃X3h, and all the above times are insulation time. There are two alloys, a total of 8 groups, and 20 wheels in each group are selected for process verification. After aging, rough turning and baking varnish treatment are carried out. The specific process is as follows:

[0057] Solution treatment: The two alloys were subjected to solution treatment at different temperatures, high temperature solution treatment at 540℃ for 6 hours and low temperature solution treatment at 520℃ for 6 hours.

[0058] Quenching: water temperature 44℃, immersion time 15 seconds, stay in water for 20 minutes, then fully cool and then aging.

[0059] Aging: For the two alloys with different chemical compositions, the aging processes are 130℃-4 hours and 170℃-4 hours respectively.

[0060] Rough processing: carried out in a constant temperature workshop at 25℃.

[0061] Paint treatment: Paint treatment performs the following process, please refer to Table 2.

[0062] Table 2

[0063] Line Furnace temperature control Base powder line (high temperature base powder) 180℃*10min Foundation powder line (low temperature foundation powder) 160℃*20min Paint line 140℃*23min Transparent powder line (transparent powder) 180℃*14min Transparent powder line (matte transparent powder) 180℃*20min

[0064] Finishing: carried out in a constant temperature workshop at 25℃.

[0065] Deformation detection and mechanical properties testing:

[0066] 1. Deformation detection: Two alloys, two solid solution processes, two aging processes, a total of 8 groups, each group selected 10 wheels for deformation detection. Each wheel number was compared and tested before and after heat treatment. Each wheel tested three data, the change in flatness, the change in ovality, and the change in the back distance size (the back distance is the distance from the rear wheel rim to the mounting plate). Deformation detection is shown in Table 3:

[0067] Table 3

[0068]

[0069] As can be seen from Table 3, the deformation amount is not closely related to the alloy composition and aging temperature. However, the flatness, ovality and back distance are highly correlated with the solution temperature. After low-temperature solution treatment, the deformation size has been significantly improved, indicating that low-temperature solution treatment has a very good effect on controlling wheel hub deformation.

[0070] 2. Mechanical properties test: Two alloys, two solid solution processes, two aging processes, a total of 8 groups, 10 hubs were selected for sampling in each group, and the sampling position was at the outer rim, because the outer rim is better cooled and the corresponding factors affected by casting defects are smaller, so it is easier to compare the direct effect of heat treatment on mechanical properties. Please refer to Table 4.

[0071] Table 4

[0072]

[0073] The following conclusions can be drawn from the data in Table 4:

[0074] 1) Under the same heat treatment process, the yield strength and tensile strength of the optimized alloy are lower than those of A356.2 alloy, but the elongation is higher than that of A356.3 alloy.

[0075] 2) For A356.2 alloy, at the same aging temperature, the yield strength, tensile strength and elongation of low-temperature solid solution decreased to a certain extent, indicating that low-temperature solid solution is not completely applicable to A356.2 alloy. This is because when the Mg content is high, low-temperature solid solution cannot completely dissolve Mg in the a-Al matrix, resulting in a reduction in the subsequent precipitation strengthening effect.

[0076] 3) However, for the optimized alloy, at the same aging temperature, the mechanical properties of low-temperature solid solution and high-temperature solid solution are almost exactly the same, indicating that the optimized alloy can perfectly match the low-temperature solid solution process.

[0077] 4) Under the same solution treatment process, as the aging temperature increases, the yield strength and tensile strength increase, but the elongation decreases, which is completely consistent with the principle of aging strengthening.

[0078] 5) Comparing A356.2+high temperature solution+low temperature aging, the process of optimizing alloy+low temperature solution+high temperature aging is shown in the two sets of data in the red box in Table 4. The yield strength, tensile strength and elongation are improved, indicating that the combined optimization of the alloy heat treatment process can greatly reduce the deformation while also slightly improving the mechanical properties.

[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A heat treatment method for a wheel hub, It is characterized in that The following steps are involved: Placing the wheel hub to be treated in a heat treatment device for low-temperature solid solution heat treatment, wherein the low-temperature solid solution heat treatment is maintained within a first temperature range for a first time; Placing the wheel hub after the solution heat treatment into water for quenching, wherein the quenching is performed in water, the quenching is maintained within a second temperature range for a second time, and the wheel hub is taken out after the quenching; The hub is subjected to an aging treatment, wherein the aging treatment is performed within a third temperature range and the aging treatment is maintained for a third time.

2. The heat treatment method according to claim 1, It is characterized in that After the low temperature solution heat treatment, the hub is placed in water within 25 seconds.

3. The heat treatment method according to claim 1, It is characterized in that The first temperature range is 480-530° C., and the first time is 4-12 hours.

4. The heat treatment method according to claim 1, It is characterized in that The second temperature range is 20-90° C., and the second time is 15-30 minutes.

5. The heat treatment method according to claim 1, It is characterized in that The third temperature range is 150-180° C., and the third time is 2-8 hours.

6. The heat treatment method according to claim 1, It is characterized in that The wheel hub to be processed is made of low-pressure cast aluminum alloy, and the low-pressure cast aluminum alloy comprises, in terms of chemical composition mass percentage: Si 6.6-7.4%; Fe<0.15%; Mg 0.20-0.30%; Cu 0.20-0.40%; Sr0.008-0.02%; Ti0.08-0.3%; Mn<0.10%; Ni, Zn<0.02%; Pb, Sn<0.01%; Zr<0.01%; Ca<0.003%.

7. The heat treatment method according to claim 6, It is characterized in that The wheel hub to be processed is prepared by the following steps: a. Adding alloy ingots and recycled materials into a furnace for smelting, deslagging in the furnace at a temperature range of 760-800° C. to form molten metal, and pouring the molten metal into a transfer bag; b. Add Mg, Ti, Sr elements into the transfer bag to adjust the chemical composition, and then perform degassing and deslagging treatment inside the transfer bag; c. Pour the molten metal into a low-pressure casting insulation furnace to perform low-pressure casting of a hub blank, and perform burr removal and riser treatment on the hub blank to obtain the hub to be processed.

8. The heat treatment method according to claim 7, It is characterized in that The Ti element is added to the transfer bag in the form of an Al-5%-Ti-1% master alloy, Mg is added in the form of pure Mg or an Al-Mg master alloy, and Sr is added in the form of Al-10% Sr.

9. The heat treatment method according to claim 7, It is characterized in that It also includes, after the molten metal in the transfer ladle is degassed and deslagging, conducting a vacuum density test on the molten metal, the test is conducted at 720-760°C to ensure that the vacuum density test requirement is 2.65g / cm3.

10. The heat treatment method according to claim 7, It is characterized in that When the wheel hub blank is cast at low pressure, a filter screen is added to the liquid inlet at the bottom of the mold, and the filter screen is only used for the low pressure casting of one wheel hub blank.