Laser composite strengthening method with high surface hardness uniformity and application

By using laser remelting with large spots, high heat inputs, and multiple rounds of laser quenching with small spots and low heat inputs on the surface of steel components, the problem of uneven laser remelting structure is solved, and the uniformity of surface hardness and corrosion resistance is achieved Improvement and expand the application scope of laser composite enhancement.

CN119020775AActive Publication Date: 2024-11-26NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411135235.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The microstructure after laser remelting is uneven, resulting in uneven surface hardness and wear-resistant corrosion resistance of steel components, limiting the application range of laser remelting strengthening.

Method used

The laser remelting is used to form a remelting layer by using large spots and high heat inputs. Then, multiple rounds of laser quenching are performed using small spots and low heat inputs on the surface of the remelting layer to form a quenching layer. The quenching spots complement each other to form overlap to compensate for thermal interference. Achieve uniform hardness.

Benefits of technology

A surface hardening layer with uniform hardness and flat surface is formed, which improves the wear and corrosion resistance of steel components and expands the application range of laser composite reinforcement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020775A_ABST
    Figure CN119020775A_ABST
Patent Text Reader

Abstract

The invention discloses a laser composite strengthening method with high surface hardness uniformity and application. The laser composite strengthening method comprises the steps that laser remelting is conducted on the surface of a metal component along a plurality of remelting channels, a remelting layer is formed, the adjacent remelting channels are in lap joint, and adjacent remelting light spots in any remelting channel are overlapped; multiple rounds of laser quenching are conducted on the surface of the remelting layer along a plurality of quenching channels to form a quenching layer, in any round, adjacent quenching channels are in lap joint, adjacent quenching light spots in any quenching channel are separated from one another, and for the quenching channel, the positions of the light spots in the multiple rounds are complementary to form overlapping. According to the laser composite strengthening method provided by the invention, the laser quenching with smaller light spot size and smaller heat input is performed on the surface of the remelting layer, and the partially overlapped quenching channel is formed through multi-round complementation, so that the thermal interference between light spots is compensated, and the surface hardening layer with uniform hardness is formed on the surface of the component.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of surface engineering technology, and in particular to a laser composite strengthening method with high surface hardness uniformity and its application, which is mainly used for preparing a surface wear-resistant and corrosion-resistant strengthening layer of key components. Background Art

[0002] Laser remelting can obtain a surface layer with ultra-fine structure, the same composition as the matrix, and complete metallurgical bonding on the surface of the steel matrix through rapid cooling, which can significantly improve the surface hardness and wear and corrosion resistance of steel components. It is considered to be a very promising surface strengthening method. However, the microstructure of the laser remelting molten pool after solidification is not uniform, and there is a high overlap rate between adjacent spots and passes during laser cladding or remelting. The spot of the latter pass has a thermal effect on the previous remelted solidified structure, resulting in uneven microstructure and performance of the remelted surface. In actual use, this unevenness will cause local wear or pitting, reducing the expected service life. This quality problem limits the application scope of laser remelting strengthening. Therefore, in order to realize the large-scale application of laser remelting, a laser surface strengthening method that can obtain a more uniform surface hardness is needed. Summary of the invention

[0003] In view of the deficiencies in the prior art, the present invention aims to provide a laser composite strengthening method and application with high surface hardness uniformity.

[0004] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0005] In a first aspect, the present invention provides a laser composite strengthening method with high surface hardness uniformity, comprising:

[0006] Using a first spot diameter and a first heat input to perform laser remelting on the surface of the metal component along a plurality of remelting paths to form a remelting layer, wherein adjacent remelting paths are overlapped and adjacent remelting spots in any remelting path overlap;

[0007] A second spot diameter and a second heat input are used to perform multiple rounds of laser quenching on the surface of the remelted layer along multiple quenching paths to form a quenched layer, wherein in any round, there is an overlap between adjacent quenching paths, adjacent quenching spots in any quenching path are separated from each other, and for the quenching path, the positions of the spots between multiple rounds are complementary to form an overlap;

[0008] Wherein, the first light spot diameter is larger than the second light spot diameter, and the first heat input is higher than the second heat input.

[0009] In a second aspect, the present invention also provides a surface-strengthened component made by the above-mentioned laser strengthening composite method, which comprises a component matrix, a remelting layer and a quenching layer stacked in sequence;

[0010] The remelting layer includes remelting spots arranged along a plurality of remelting paths, and the quenching layer includes quenching spots arranged along a plurality of quenching paths. There is overlap between adjacent remelting paths, there is overlap between adjacent remelting spots in any remelting path, there is overlap between adjacent quenching paths, the quenching spots in any quenching path are divided into a plurality of rounds, the quenching spots in any round are separated from each other, and the positions of the quenching spots in a plurality of rounds are complementary to form overlaps.

[0011] Based on the above technical solution, compared with the prior art, the beneficial effects of the present invention at least include:

[0012] The laser composite strengthening method provided by the present invention performs laser quenching with a smaller spot size and smaller heat input on the surface of the remelting layer, and forms a quenching path with partial overlap through multiple rounds of complementarity, thereby compensating for the thermal interference between the spots, thereby forming a surface hardened layer with uniform hardness on the surface of the component, and the surface flatness of the formed strengthening layer is high.

[0013] The above description is only an overview of the technical solution of the present invention. In order to enable those skilled in the art to more clearly understand the technical means of the present application and implement them according to the contents of the specification, the following is a description of the preferred embodiments of the present invention in conjunction with detailed drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a schematic diagram of the relationship between the spot path and the spot position of the laser composite strengthening method provided by a typical implementation case of the present invention;

[0015] Figure 2 It is a schematic diagram of the distribution of surface hardness test points provided by some typical implementation cases and comparative cases of the present invention;

[0016] Figure 3 This is a hardness distribution test diagram of the surface strengthening layer provided by a typical comparative case of the present invention;

[0017] Figure 4 This is a hardness distribution test diagram of the surface strengthening layer provided by a typical implementation case of the present invention;

[0018] Figure 5 is a hardness distribution test diagram of a surface strengthening layer provided by another typical embodiment of the present invention;

[0019] Figure 6 This is a hardness distribution test diagram of the surface strengthening layer provided by another typical implementation case of the present invention. DETAILED DESCRIPTION

[0020] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution, its implementation process and principle will be further explained as follows.

[0021] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0022] Moreover, relational terms such as “first” and “second” are merely used to distinguish one component or method step from another with the same name, but do not necessarily require or imply any such actual relationship or order between these components or method steps.

[0023] The embodiment of the present invention provides a laser composite strengthening method with high surface hardness uniformity, which comprises the following steps:

[0024] Using a first spot diameter and a first heat input to perform laser remelting on the surface of the metal component along a plurality of remelting paths to form a remelting layer, wherein adjacent remelting paths are overlapped and adjacent remelting spots in any remelting path overlap;

[0025] A second spot diameter and a second heat input are used to perform multiple rounds of laser quenching on the surface of the remelted layer along multiple quenching paths to form a quenched layer, wherein in any round, there is an overlap between adjacent quenching paths, adjacent quenching spots in any quenching path are separated from each other (no overlap occurs), and for the quenching path, the spot positions between multiple rounds complement each other to form an overlap;

[0026] Wherein, the first light spot diameter is larger than the second light spot diameter, and the first heat input is higher than the second heat input.

[0027] The main technical means of the above technical scheme is to prepare a remelted layer on the surface of the steel component to be strengthened under the conditions of large spot and high heat input, and then use a small spot and lower heat input for quenching to obtain a high-hardness and uniform surface hardened layer. The purpose is to provide a laser composite strengthening technology that can achieve high and uniform hardness of the surface remelted layer, which can replace the traditional laser cladding or remelting technology and is used for the surface strengthening of steel wear-resistant and corrosion-resistant components.

[0028] It is worth noting that in the present invention, the diameter of the quenching spot is smaller than the diameter of the remelting spot, and the overlapping arrangement is achieved by a single-round discrete and multiple-round complementary method. This is because there is a high overlap rate between adjacent spots and passes during laser cladding or remelting, and the spot of the later pass has a thermal effect on the previous remelted solidified structure, which leads to unevenness. The laser quenching in the present invention compensates for the above-mentioned unevenness and strengthens it, so the quenching spot needs to be smaller in size; in addition, since two quenching spots adjacent in time will cause heat superposition and affect each other, it is not appropriate to use a single-round overlapping method to directly complete laser quenching, but requires multiple rounds of overlapping methods to complete it.

[0029] For detailed spot distribution, see Figure 1 As shown, in some embodiments, the quenching track is arranged in parallel with the remelting track, and the center line of the quenching track runs along the overlapping seam of two adjacent remelting tracks; the overlapping seam refers to the common tangent line of the edges of multiple remelting spots in the adjacent subsequent remelting track, and the common tangent line is located on the side close to the previous remelting track.

[0030] In some embodiments, N represents the number of laser quenching rounds, L represents the center distance between adjacent quenching spots in any quenching path in any round, and P represents the center offset distance between quenching spots in adjacent rounds in any quenching path, then:

[0031] P = L / N;

[0032] Wherein, L>L0, L0 refers to the second light spot diameter.

[0033] In some embodiments, the number of rounds of laser quenching is 2-3 rounds.

[0034] In some embodiments, in any one of the quenching tracks, the overall overlap rate of the quenching spots of all rounds is 40-60%.

[0035] In some embodiments, during the laser remelting, the overlap rate of adjacent remelting tracks is 60-70%, and the overlap rate of light spots in any remelting track is 60-80%.

[0036] In some embodiments, during the laser quenching, the overlap rate between adjacent quenching lanes is 20-30%.

[0037] In some embodiments, the first light spot has a diameter of 0.5-2.0 mm.

[0038] In some embodiments, the second spot diameter is 40-60% of the first spot diameter.

[0039] As for other condition parameters, such as heat input controlled by current, pulse width and frequency, they can be adaptively adjusted for different materials, different cladding thicknesses, etc., and you can refer to many existing technologies or experiment with the process window yourself; not only that, the irradiation frequency of remelting and quenching can also be adaptively adjusted to match the scanning speed. The main purpose is to control the overlap rate.

[0040] In some embodiments, the last spot of the laser remelting and the laser irradiation are completely outside the preset strengthening area of ​​the metal component to avoid a complete molten pool remaining.

[0041] The second aspect of the embodiment of the present invention further provides a surface-strengthened component made by the laser strengthening composite method in any of the above embodiments, which comprises a component matrix, a remelting layer and a quenching layer stacked in sequence;

[0042] The remelting layer includes remelting spots arranged along a plurality of remelting paths, and the quenching layer includes quenching spots arranged along a plurality of quenching paths. There is overlap between adjacent remelting paths, there is overlap between adjacent remelting spots in any remelting path, there is overlap between adjacent quenching paths, the quenching spots in any quenching path are divided into a plurality of rounds, the quenching spots in any round are separated from each other, and the positions of the quenching spots in a plurality of rounds are complementary to form overlaps.

[0043] As some typical examples of the above-mentioned technical solutions, the present invention provides a laser composite strengthening method that combines laser surface large-spot high-heat input remelting with small-spot low-heat input quenching, which can be used for surface wear and corrosion protection of metal components such as large-size hot working molds, especially steel components. The exemplary main steps are: first, clean the surface of the steel component to remove surface stains and oxide layers, and remelt the surface under the conditions of large spot and high heat input. The laser equipment, current, scanning speed, pulse frequency, pulse width, spot size, etc. can be flexibly selected, with a pass overlap rate of 60-70% and a spot overlap rate of 60-80%; then use a small spot and lower heat input to quench the tangent area of ​​the remelting spot. The quenching spot diameter is 40-60% of the remelting spot, and it is divided into 2-3 rounds. The spots in any pass of each round are discontinuous and have intervals to ensure the quenching effect, and the next round or multiple rounds of spots fill the interval area to form a complementary, and finally the spot overlap rate of the multiple rounds of overlapping passes is 40-60%, and a surface hardening layer with uniform hardness is obtained. The advantage of the above technical solution is that it can prepare a remelting quenching strengthening layer with high and uniform microstructure, surface hardness and corrosion resistance, and hardened layer thickness, with a flat surface and low energy consumption.

[0044] Exemplarily, the main component of the components used in the embodiments of the present invention can be low alloy steel or stainless steel, but it is not limited to this. Metal materials with similar properties that can be subjected to surface laser quenching and strengthening treatment can utilize the technical solution provided by the present invention, such as nickel alloys, titanium alloys, aluminum alloys, high alloy steels, etc. Of course, the spot size and overlap arrangement of different materials should meet the above requirements, but some other condition parameters such as laser power need to be adaptively adjusted.

[0045] The technical solution of the present invention is further described in detail below through several embodiments and in conjunction with the accompanying drawings. However, the selected embodiments are only used to illustrate the present invention, and do not limit the scope of the present invention.

[0046] Comparative Example 1

[0047] The surface of the H13 hot working die steel plate with a thickness of 10 mm was mechanically polished to remove surface stains and oxide layer, and then rinsed with water and alcohol in turn and then blown dry;

[0048] The laser remelting current is 50A, the scanning rate is 108mm / min, the spot diameter is 0.6mm, the frequency is 10Hz, and the pulse width is 6ms to achieve a 70% overlap rate; the overlap rate between passes is 60%; the remelting path is as follows Figure 1 As shown, the final light spot ends outside the workpiece.

[0049] The surface hardness of the remelting spot was measured using a micro Vickers hardness tester with a load of 50 g and a holding time of 10 s. The microhardness indentation positions were measured along the diameter of the remelting spot at intervals of 0.03 mm. Figure 2 As shown, there are 100 points in total, and the hardness distribution is obtained as Figure 3 In the figure, 1 to 10 refer to a row of test points from top to bottom, and the vertical axis is the hardness of each row from left to right.

[0050] Example 1

[0051] This embodiment adds a laser quenching process based on the comparative example 1, which is as follows:

[0052] The surface of the H13 hot working die steel plate with a thickness of 10 mm was mechanically polished to remove surface stains and oxide layer, and then rinsed with water and alcohol in turn and then blown dry;

[0053] The laser remelting current is 50A, the scanning rate is 108mm / min, the spot diameter is 0.6mm, the frequency is 10Hz, and the pulse width is 6ms to achieve a 70% overlap rate; the overlap rate between passes is 60%; the remelting path is as follows Figure 1 As shown, the final light spot ends outside the workpiece.

[0054] The laser quenching current was 15A, the scanning rate was 190mm / min, the spot diameter was 0.3mm, the frequency used was 10Hz, and the pulse width was 8ms, so that the quenching spots did not overlap; the overlap rate between passes was 24%; two rounds of laser quenching were performed, and the paths of the quenching passes of the two were consistent, both moving along the joints of the remelting spots, but the offset of the spot along the quenching pass was half of the quenching spot spacing;

[0055] The surface hardness of the remelting spot was measured using a micro Vickers hardness tester with a load of 50 g and a holding time of 10 s. The hardness distribution was obtained along the diameter of the remelting spot at intervals of 0.03 mm. Figure 4 shown.

[0056] Comparative Example 2

[0057] This comparative example is substantially the same as Example 1, except that:

[0058] When laser quenching is performed, it is not divided into multiple rounds, but all quenching spots are irradiated in one round, and the irradiation frequency remains unchanged.

[0059] The result is that the surface hardness is low, and the average hardness is reduced by 10-15% compared with Example 1. The reason is that the latter laser pulse is emitted before the high temperature caused by the previous pulse has not dropped, which delays the temperature drop and thus reduces the quenching effect.

[0060] Comparative Example 3

[0061] This comparative example is substantially the same as Example 1, except that:

[0062] During laser quenching, the quenching path does not run along the joints of the remelted spots, but runs along the center of the remelted spots.

[0063] The consequence is that the hardness of the overlap zone is low, and the gap with the center zone increases. The reason is that the hardness of the joint zone itself is low, and without further quenching, its hardness is even greater than that of the center zone that has undergone secondary quenching.

[0064] This shows that making the quenching path run along the joints of the remelted spots is a key factor in using the arrangement of quenching spots to compensate for the hardness non-uniformity.

[0065] Example 2

[0066] The surface of the H13 hot working die steel plate with a thickness of 6 mm was mechanically polished to remove surface stains and oxide layer, and then rinsed with water and alcohol in turn and then blown dry;

[0067] The laser remelting current is 45A, the scanning rate is 108mm / min, the spot diameter is 0.6mm, the frequency is 10Hz, and the pulse width is 8ms to achieve a 70% overlap rate; the overlap rate between passes is 60%; the remelting path is as follows Figure 1 As shown, the final light spot ends outside the workpiece.

[0068] The laser quenching current is 12A, the scanning rate is 190mm / min, the spot diameter is 0.3mm, the frequency is 10Hz, and the pulse width is 7ms, so that the quenching spots do not overlap; the overlap rate between passes is 24%;

[0069] Two rounds of quenching were performed, and the starting position offset between the two rounds was half of the quenching spot spacing;

[0070] The surface hardness of the remelting spot was measured using a micro Vickers hardness tester with a load of 50 g and a holding time of 10 s. The hardness distribution was obtained along the diameter of the remelting spot at intervals of 0.03 mm. Figure 5 shown.

[0071] Example 3

[0072] The surface of the 8mm thick H13 hot working die steel plate was mechanically polished to remove surface stains and oxide layer, and then rinsed with water and alcohol in turn and then blown dry;

[0073] The laser remelting current is 40A, the scanning rate is 108mm / min, the spot diameter is 0.6mm, the frequency is 10Hz, and the pulse width is 8ms to achieve a 70% overlap rate; the overlap rate between passes is 60%; the remelting path is as follows Figure 1 As shown, the final light spot ends outside the workpiece.

[0074] The laser quenching current was 10A, the scanning rate was 190mm / min, the spot diameter was 0.3mm, the frequency was 10Hz, and the pulse width was 10ms, so that the quenching spots did not overlap; the overlap rate between passes was 24%;

[0075] Two rounds of quenching were performed, and the starting position offset between the two rounds was half of the quenching spot spacing;

[0076] The surface hardness of the remelting spot was measured using a micro Vickers hardness tester with a load of 50 g and a holding time of 10 s. The hardness distribution was obtained along the diameter of the remelting spot at intervals of 0.03 mm. Figure 6 shown.

[0077] Example 4

[0078] This embodiment is substantially the same as the embodiment 3, with the main difference being that during laser quenching, the scanning rate is 190 mm / min, the frequency used is 15 Hz, the spot diameter is 0.2 mm, and the spot spacing is 0.21 mm; three rounds of quenching are performed, and the starting position offset of each round of quenching is 1 / 3 of the spot spacing.

[0079] The obtained surface composite strengthening layer still has a relatively high hardness value and hardness uniformity.

[0080] Example 5

[0081] This embodiment is substantially the same as Embodiment 3, with the main difference being that the substrate is replaced with stainless steel, model TC4 titanium alloy.

[0082] When other conditions remain unchanged, the obtained surface composite strengthening layer still has a high hardness value and hardness uniformity.

[0083] Example 6

[0084] This embodiment is substantially the same as Embodiment 3, with the main difference being that the substrate is replaced with 3003 aluminum alloy.

[0085] When other conditions remain unchanged, the obtained surface composite strengthening layer still has a high hardness value and hardness uniformity.

[0086] Based on the above embodiments and comparative examples, it can be clearly seen that the laser composite strengthening method provided in the embodiments of the present invention compensates for the thermal interference between the light spots by performing laser quenching with a smaller spot size and smaller heat input on the surface of the remelting layer, and forms a quenching path with partial overlap through multiple rounds of complementarity, thereby forming a surface hardened layer with uniform hardness on the surface of the component, and the formed strengthening layer has high surface flatness and low energy consumption in the surface strengthening process.

[0087] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A laser composite strengthening method with high surface hardness uniformity, It is characterized in that include: Using a first spot diameter and a first heat input to perform laser remelting on the surface of the metal component along a plurality of remelting paths to form a remelting layer, wherein adjacent remelting paths are overlapped and adjacent remelting spots in any remelting path overlap; A second spot diameter and a second heat input are used to perform multiple rounds of laser quenching on the surface of the remelted layer along multiple quenching paths to form a quenched layer, wherein in any round, there is an overlap between adjacent quenching paths, adjacent quenching spots in any quenching path are separated from each other, and for the quenching path, the positions of the spots between multiple rounds are complementary to form an overlap; Wherein, the first light spot diameter is larger than the second light spot diameter, and the first heat input is higher than the second heat input.

2. The laser strengthening composite method according to claim 1, It is characterized in that The quenching track is arranged in parallel with the remelting track, and the center line of the quenching track runs along the overlapping seam of two adjacent remelting tracks; the overlapping seam refers to the common tangent line of the edges of multiple remelting spots in the adjacent subsequent remelting track, and the common tangent line is located on the side close to the previous remelting track.

3. The laser strengthening composite method according to claim 2, It is characterized in that N represents the number of laser quenching rounds, L represents the center distance between adjacent quenching spots in any quenching path in any round, and P represents the center offset distance between quenching spots in adjacent rounds in any quenching path. Then: P = L / N; Among them, L>L 0 , L 0 It refers to the second spot diameter.

4. The laser enhanced composite method according to claim 3, It is characterized in that The number of rounds of laser quenching is 2-3 rounds.

5. The laser enhanced composite method according to claim 3, It is characterized in that In any of the quenching tracks, the overall overlap rate of the quenching spots of all rounds is 4060%.

6. The laser enhanced composite method according to claim 1, It is characterized in that In the laser remelting, the overlap rate of adjacent remelting tracks is 60-70%, and the overlap rate of light spots in any remelting track is 60-80%.

7. The laser enhanced composite method according to claim 6, It is characterized in that During the laser quenching, the overlap rate between adjacent quenching paths is 20-30%.

8. The laser enhanced composite method according to claim 1, It is characterized in that The diameter of the first light spot is 0.52.0 mm; And / or, the diameter of the second light spot is 40-60% of the diameter of the first light spot.

9. The laser enhanced composite method according to claim 1, It is characterized in that The last light spot of the laser remelting and the laser irradiation is completely outside the preset strengthening area of ​​the metal component.

10. A surface-reinforced component obtained by the laser reinforcing composite method according to any one of claims 1 to 9, It is characterized in that It includes a component matrix, a remelting layer and a quenching layer which are stacked in sequence; The remelting layer includes remelting spots arranged along a plurality of remelting paths, and the quenching layer includes quenching spots arranged along a plurality of quenching paths. There is overlap between adjacent remelting paths, there is overlap between adjacent remelting spots in any remelting path, there is overlap between adjacent quenching paths, the quenching spots in any quenching path are divided into a plurality of rounds, the quenching spots in any round are separated from each other, and the positions of the quenching spots in a plurality of rounds are complementary to form overlaps.

Citation Information

Patent Citations

  • Manufacturing method of strengthened valve tappet

    CN104862694A

  • Adjustable wide-band bidirectional symmetrical powder-feeding laser melting-painting nozzle

    CN1319459A

  • Laser Cladding on Low Heat Resistant Substrates

    US20080226843A1

  • High entropy alloy powder for laser cladding and application method thereof

    US20220097133A1

  • High speed and power energy beam welding method

    WO1996033041A1