Preparation method and application of CsAg2I3 single-crystal microwire material
The ultra-long growth of CsAg2I3 single crystal micron wires was achieved by low-temperature solvent growth under conditions below 60°C, which solved the problem of the size of silver-based perovskite single crystal micron wires being too short, and high-quality CsAg2I3 single crystal micron wire and applied to photoconductive sensors, it has the advantages of simple operation and large-scale preparation.
Patent Information
- Application Number
- CN202411121483.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, silver-based perovskite single crystal microwires are too short to obtain high-quality single crystal materials with ideal size, morphology and photoelectric properties.
Using low-temperature solvent growth method, using organic mixed solvent as crystal growth precursor solution, the molar ratio, solvent ratio and centrifugal conditions of CsI and AgI can achieve high-quality ultra-length of CsAg2I3 single crystal micron wires under conditions below 60°C. Grow.
While ensuring high quality of single crystals, ultra-long growth is achieved, CsAg2I3 single crystal micron wires with a length of up to centimeters are prepared, and CsAg2I3 single crystal micron wire photoconductivity sensor is prepared through low-temperature annealing treatment, with a simple process. , the advantages of efficient and easy operation of the process and large-scale preparation.
Smart Images

Figure CN119020847A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of new material preparation, and specifically relates to a preparation method and application of a CsAg2I3 single crystal micron wire material. Background Art
[0002] Inorganic halide perovskites have attracted extensive attention for their excellent optoelectronic properties, such as wide emission spectra, large Stokes shifts, adjustable band gaps, and ultra-long carrier diffusion lengths. In recent years, single-crystalline perovskites without grain boundary defects have shown enhanced properties in terms of carrier migration. As a non-toxic and low-cost CsAg2I3 single-crystalline perovskite material, it has expanded the exploration of new lead-free halides. The optoelectronic properties of single crystals are affected by their size and morphology, so pure phase, high-quality perovskite single crystals can further obtain ideal optoelectronic properties. At present, silver-based perovskite single crystal microwires have the problem of being too short in size, and it is urgent to find an effective method to obtain single crystals with ideal size, morphology, and optoelectronic properties. Summary of the invention
[0003] Purpose of the invention: The technical problem to be solved by the present invention is to provide a method for preparing ultra-long CsAg2I3 single crystal perovskite material grown by low-temperature solvent in view of the shortcomings of the prior art. The preparation process is simple and easy to operate. The method uses an organic mixed solvent as a crystal growth precursor solution and can achieve high-quality ultra-long growth of single crystals under experimental conditions below 60°C.
[0004] In order to solve the above technical problems, the present invention discloses a method for preparing a CsAg2I3 single crystal microwire material, the specific steps of which are:
[0005] S1. dissolving CsI and AgI in a solvent to obtain a precursor solution;
[0006] S2. Purifying the precursor solution obtained in S1;
[0007] S3. Add the purified precursor solution in S2 into container A, and place container A into container B filled with anti-solvent, and keep warm to grow CsAg2I3 single crystal microwires.
[0008] Wherein, in said S1, the specific steps are: adding CsI and AgI into a solvent, stirring at 50-60° C. for 1.5-2 h to obtain a precursor solution;
[0009] Preferably, in S1, the specific steps are: adding CsI and AgI into a solvent, and stirring at 60° C. for 2 hours to obtain a precursor solution.
[0010] Wherein, the molar ratio of CsI to AgI is 1:(0.5-2); the solvent is a mixed solvent of dimethylformamide and dimethyl sulfoxide; the molar ratio of dimethylformamide to dimethyl sulfoxide is (1-5):1;
[0011] Preferably, the molar ratio of CsI to AgI is 1:2; and the molar ratio of dimethylformamide to dimethyl sulfoxide is 1:1.
[0012] Wherein, in said S2, the specific steps are: placing the precursor solution obtained in S1 into a centrifuge, centrifuging at 8500-9000 rpm / min for 5-10 min, and taking the upper clear layer as the purified precursor solution;
[0013] Preferably, in S2, the specific steps are: placing the precursor solution obtained in S1 into a centrifuge, centrifuging at 9000 rpm / min for 5 minutes, and taking the upper clear layer as the purified precursor solution.
[0014] Among them, in S3, the A container is a beaker sealed with aluminum foil and paraffin film; the B container is a blue-capped bottle; the anti-solvent is methanol;
[0015] Preferably, in S3, the aluminum foil in the container A has 3 to 8 small holes with the same pore size; the pore size of the small holes is 140 to 160 μm;
[0016] More preferably, in S3, there are four small holes with the same pore size on the aluminum foil in the container A; the pore size of the small holes is 150 μm;
[0017] More preferably, the capacity of the blue-capped bottle is 500 ml; 30-40 ml of methanol is injected into the blue-capped bottle; and the content of the precursor solution in the A container is 2 ml.
[0018] Wherein, in S3, the conditions of the heat preservation growth process are heat preservation at 50-70° C. for 20-40 hours;
[0019] Preferably, in S3, the condition of the heat preservation growth process is heat preservation at 60° C. for 30 hours.
[0020] Specifically, in some embodiments of the present invention, after the CsAg2I3 single crystal micron wire is prepared by the above-mentioned preparation method of the CsAg2I3 single crystal micron wire material, the CsAg2I3 single crystal micron wire is prepared by applying silver paste to both ends of the CsAg2I3 single crystal micron wire and performing low temperature annealing treatment to obtain a CsAg2I3 single crystal micron wire photoconductive sensor;
[0021] Preferably, the conditions of the low-temperature annealing process are an annealing temperature of 60-80° C. and an annealing time of 40-60 min.
[0022] Beneficial effects: The present invention can adjust the nucleation and crystal growth process in the precursor solution by controlling the precursor concentration, diffusion rate and other conditions of the perovskite antisolvent, and achieve ultra-long growth of single crystals while ensuring the high quality of micron-wire single crystals. In addition, the method adopted by the present invention is a low-temperature solution method, which has the advantages of simple process, efficient process, easy operation and large-scale preparation. Its preparation process can grow ultra-long centimeter-level CsAg2I3 single crystal micron wires. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.
[0024] Figure 1 This is an optical photograph of CsAg2I3 single crystal microwires prepared in Example 1 of the present invention;
[0025] Figure 2 The XRD spectrum of CsAg2I3 single crystal microwire powder prepared in Example 1 of the present invention;
[0026] Figure 3 The high-resolution TEM and electron diffraction patterns of the CsAg2I3 single crystal micrometer line prepared in Example 1 of the present invention;
[0027] Figure 4 The absorption spectrum of the CsAg2I3 single crystal micrometer wire prepared in Example 1 of the present invention;
[0028] Figure 5 It is the IT spectrum of the blue light response of the CsAg2I3 single crystal microwire prepared in Example 1 of the present invention;
[0029] Figure 6 This is an optical photograph of CsAg2I3 single crystal microwires prepared in Example 2 of the present invention;
[0030] Figure 7 This is an optical photograph of CsAg2I3 single crystal microwires prepared in Example 3 of the present invention;
[0031] Figure 8 This is an optical photograph of the CsAg2I3 single crystal microwire prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0034] Embodiment 1:
[0035] A preparation method and application of CsAg2I3 single crystal microwire material, comprising the following steps:
[0036] S1. Preparation of precursor solution: 0.26 g of CsI and 0.47 g of AgI (CsI:AgI molar ratio is 1:2) were mixed and added into a mixed solvent of DMF (1 ml) and DMSO (1 ml); stirred for 2 h in an oil bath at 60°C until the solution became homogeneous and transparent to obtain a precursor solution;
[0037] S2. The prepared precursor solution was placed in a centrifuge and centrifuged at 9000 rpm / min for 5 min, and the supernatant was taken;
[0038] S3. Quickly put the supernatant into a small beaker and seal it with aluminum foil and paraffin film as container A. Punch 4 small holes (diameter ~150um) in the aluminum foil and paraffin film. Inject 30ml of methanol into a blue-capped bottle as container B. Put container A into container B and seal it at 60℃ for 30h to obtain CsAg2I3 single crystal microwires.
[0039] S4. Apply the purchased silver paste to both ends of the CsAg2I3 single crystal microwire, and anneal at 80°C for 60 minutes to allow the silver paste and the microwire to form a good conductive contact, thereby preparing a CsAg2I3 single crystal photoconductive sensor.
[0040] The optical photograph of the CsAg2I3 single crystal prepared in this example is shown in Figure 1 As shown in the figure, it can be seen that the longest CsAg2I3 single crystal can reach 3cm;
[0041] The X-ray diffraction pattern of the CsAg2I3 single crystal prepared in this example is as follows Figure 2 The powder used for X-ray characterization is prepared by grinding single crystal microwires; Figure 2 It can be seen that CsAg2I3 material (PDF#01-072-9860) was successfully prepared. Figure 3 High-resolution TEM and selected-area electron diffraction patterns show that CsAg2I3 is a single-crystalline material;
[0042] The absorption spectrum of the CsAg2I3 single crystal microwire prepared in this example is as follows Figure 4 As shown, the material has a clear absorption cutoff edge at 430nm, indicating that the single crystal material may have photoelectric response ability in the blue light region;
[0043] The photoelectric response spectrum of the CsAg2I3 single crystal microwire prepared in this example is as follows Figure 5 As shown, the device exhibited stable photoelectric response ability under 430nm blue light irradiation under 2V bias.
[0044] Embodiment 2:
[0045] A preparation method and application of CsAg2I3 single crystal microwire material; different from Example 1 in that the ratio of raw materials used in step S1 is different, the precursor solution contains 0.78g of CsI and 0.47g of AgI (CsI:AgI molar ratio is 3:2), and the other conditions are the same.
[0046] The optical photograph of the CsAg2I3 single crystal prepared in this example is shown in Figure 6 As shown in the figure, it can be seen that the longest CsAg2I3 single crystal microwire can reach 1.4cm.
[0047] Embodiment 3:
[0048] A preparation method and application of CsAg2I3 single crystal microwire material; different from Example 1 in that the ratio of raw materials used in step S1 is different, the precursor solution contains 0.52g of CsI and 0.24g of AgI (CsI:AgI molar ratio is 2:1), and the other conditions are the same.
[0049] The optical photograph of the CsAg2I3 single crystal prepared in this example is shown in Figure 7 As shown in the figure, it can be seen that the longest CsAg2I3 single crystal microwire can reach 1.2cm.
[0050] Embodiment 4:
[0051] A preparation method and application of CsAg2I3 single crystal micrometer wire material; different from Example 1 in that the growth temperature in step S1 is different, container A is placed in container B and sealed at 50°C for 30 hours to obtain CsAg2I3 single crystal micrometer wires, and the diffusion rate of the antisolvent can be controlled by changing the growth temperature, thereby achieving control of the nucleation and growth rate, and the other conditions are the same.
[0052] The optical photograph of the CsAg2I3 single crystal prepared in this example is shown in Figure 8 As shown in the figure, it can be seen that the longest CsAg2I3 single crystal microwire can reach 1.8 cm.
[0053] The present invention provides a method for preparing and applying a CsAg2I3 single crystal microwire material. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.
Claims
1. A method for preparing CsAg2I3 single crystal microwire material, characterized in that: The specific steps are: S1. dissolving CsI and AgI in a solvent to obtain a precursor solution; S2. Purifying the precursor solution obtained in S1; S3. Add the purified precursor solution in S2 into container A, and place container A into container B filled with anti-solvent, and keep warm to grow CsAg2I3 single crystal microwires.
2. The preparation method according to claim 1, characterized in that: In the above S1, the specific steps are: adding CsI and AgI into a solvent, and stirring at 50-60° C. for 1.5-2 hours to obtain a precursor solution.
3. The preparation method according to claim 2, characterized in that: The molar ratio of CsI to AgI is 1:(0.5-2); the solvent is a mixed solvent of dimethylformamide and dimethyl sulfoxide; the molar ratio of dimethylformamide to dimethyl sulfoxide is (1-5):
1.
4. The preparation method according to claim 1, characterized in that: In said S2, the specific steps are: putting the precursor solution obtained in S1 into a centrifuge, centrifuging at 8500-9000 rpm / min for 5-10 min, and taking the upper clear layer as the purified precursor solution.
5. The preparation method according to claim 1, characterized in that: In S3, the A container is a beaker sealed with aluminum foil and paraffin film; the B container is a blue-capped bottle; and the anti-solvent is methanol.
6. The preparation method according to claim 5, characterized in that: In S3, there are 3 to 8 small holes with the same pore size on the aluminum foil in the A container; the pore size of the small holes is 140 to 160 μm.
7. The preparation method according to claim 1, characterized in that: In S3, the heat preservation growth process is carried out at 50-70° C. for 20-40 hours.
8. The CsAg2I3 single crystal microwire material prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the CsAg2I3 single crystal microwire material prepared by the preparation method according to any one of claims 1 to 7 in the preparation of a photoconductive sensor.
10. The use according to claim 9, characterized in that: The specific steps of the application are: applying silver paste to both ends of the CsAg2I3 single crystal micrometer wire, performing low temperature annealing treatment, and preparing the CsAg2I3 single crystal micrometer wire photoconductive sensor.