Preparation method of self-pumping bionic fiber membrane and application of self-pumping bionic fiber membrane in antibacterial dressing
By preparing a self-pumped bionic fiber membrane with a double-layer structure in electrospinning production, combining modified non-woven fabrics and hydrophobic modified slurry, the problem of insufficient fiber membrane performance in the prior art is solved, and the antibacterial dressing is realized Excellent effect and unidirectional fluid drainage for diabetic wound healing.
Patent Information
- Application Number
- CN202411515765.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is difficult to prepare self-pumped bionic fiber membranes with excellent hydrophilic and hydrophobic properties in electrospinning production, and their application effects in antibacterial dressings are poor.
By drying the bio-based polyamide pretreatment and mixing it with m-cresol and hydrophobic modified slurry, an electrospinning technology is used to form a self-pumping bionic fiber membrane with a double-layer structure on the modified nonwoven fabric, combined with alkalization The non-woven fabric is modified with etherification to form a hydrophilic liquid absorbing layer and a hydrophobic drainage layer, enhancing the antibacterial properties of the fiber membrane.
The preparation of self-pumped bionic fiber membranes is realized, with excellent unidirectional liquid discharge and antibacterial properties, and is suitable for diabetic wound healing, significantly improving the antibacterial effect of the dressing.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrostatic spinning production, and specifically relates to a method for preparing a self-pumping bionic fiber membrane and application of the same in antibacterial dressings. Background Art
[0002] Bionic fiber membrane is a high-performance material that simulates biological structures and functions in nature. It achieves functions such as unidirectional moisture conduction, rapid moisture absorption and evaporation by imitating certain specific structures in organisms (such as capillary effect, wetting effect and transpiration effect).
[0003] Self-pumping bionic fiber membrane is a type of material with unidirectional moisture conduction properties. Its design principles include differential capillary effect, wettability gradient effect, bionic transpiration effect, etc. There are many directional water transport phenomena based on gradient wettability in nature. For example, water can be transported in a directional manner on spider silk, water bird beaks, cactus thorns, and the back of desert beetles. In recent years, with the continuous development of electrospinning technology, Janus fiber membranes based on asymmetric structures have attracted much attention and research.
[0004] Janus fiber membrane is a composite material with an asymmetric structure, usually with two different chemical compositions or physical properties, distributed on both sides or in different regions of the material. This structure makes Janus fiber membranes useful in many fields, such as drug delivery, oil-water separation, sensors, etc. In general, the number of layers and surface properties of Janus fiber membranes can be designed according to their application purpose and functional requirements, from simple double-layer structures to more complex multi-layer structures. Summary of the invention
[0005] Based on the research of the above-mentioned prior art, the present invention has developed a method for preparing a self-pumping bionic fiber membrane and its application in antibacterial dressings. The present invention utilizes electrospinning technology to stretch a hydrophobic electrospinning precursor liquid into nanofibers and collect them on a modified non-woven fabric with excellent hydrophilicity to obtain a self-pumping bionic fiber membrane, forming a fiber membrane structure with opposite properties on both sides. At the same time, the present invention further improves the hydrophilicity and hydrophobicity of the self-pumping bionic fiber membrane by improving the preparation method. Finally, the present invention applies the prepared self-pumping bionic fiber membrane to the field of dressings, and at the same time exhibits excellent antibacterial (against Escherichia coli and Staphylococcus aureus) properties.
[0006] The purpose of the present invention can be achieved through the following technical solutions: A method for preparing a self-pumping bionic fiber membrane comprises the following steps: The bio-based polyamide is dried and pretreated, and the pretreated bio-based polyamide is added to the meta-cresol with stirring, and then stirred at 35-40°C for 2-3 hours, and then the hydrophobic modified slurry is added thereto with stirring, and stirred at room temperature for 20-30 minutes to obtain an electrospinning precursor solution, and the electrospinning precursor solution is stretched into nanofibers and collected on a modified non-woven fabric. After completion, a self-pumping bionic fiber membrane is obtained.
[0007] Furthermore, the usage ratio of the meta-cresol, the pretreated bio-based polyamide and the hydrophobically modified slurry is 10 mL: 4-5 g: 12-15 mL.
[0008] Further, the hydrophobically modified slurry is prepared by the following steps: Add 5-difluoromethoxy-2-mercapto-1H-benzimidazole to anhydrous ethanol, stir to dissolve, then add dichloromethane and vinyltrimethoxysilane, stir and mix for 30 to 40 minutes after the addition, then add 2,2-dimethoxyphenylacetophenone and triethylenetetramine, react under 30W ultraviolet light for 20 to 25 minutes to obtain a fluorine-containing silane solution, then add polypropylene to the fluorine-containing silane solution, stir at high speed for 25 to 30 minutes to obtain a hydrophobically modified slurry.
[0009] Furthermore, the dosage ratio of anhydrous ethanol, 5-difluoromethoxy-2-mercapto-1H-benzimidazole, dichloromethane, vinyltrimethoxysilane, 2,2-dimethoxyphenylacetophenone, triethylenetetramine and polypropylene is 40mL: 0.22-0.23g: 60mL: 11.5-12.0mL: 0.02g: 0.01g: 3.1-3.2g.
[0010] Furthermore, the electrospinning process parameters are as follows: the spinning box temperature is 22-28°C, the relative humidity of the spinning box is 30%-40%, the injection speed is 1.5 mL / h, the voltage is 18 kV, the electrospinning time is 5 h, the electrospinning collection distance is 15 cm, and the effective electrospinning area on the modified non-woven fabric is controlled at 300 cm 2 .
[0011] Furthermore, the modified nonwoven fabric is prepared by the following steps: The PP non-woven fabric was immersed in a sodium hydroxide solution and placed at 35 to 40°C for alkalization for 30 to 40 minutes. After completion, an alkalized non-woven fabric was obtained. The alkalized non-woven fabric was then immersed in a sodium chloroacetate-isopropanol aqueous solution and placed at 70 to 80°C for etherification for 30 to 40 minutes. After completion, an etherified non-woven fabric was obtained. The etherified non-woven fabric was then immersed in an isopropanol aqueous solution, and a phosphoric acid aqueous solution with a mass fraction of 85% was added dropwise to adjust the pH of the system to 6.5 to 7.0. After completion, the neutralized non-woven fabric was obtained by constant temperature stirring for 30 to 40 minutes. The neutralized non-woven fabric was then rinsed three times with an isopropanol aqueous solution and deionized water, and then dried for 30 to 40 minutes, taken out, and cooled to room temperature to obtain a modified non-woven fabric.
[0012] Furthermore, the sodium hydroxide solution is prepared by the following steps: adding sodium hydroxide to deionized water, wherein the amount ratio of deionized water to sodium hydroxide is 100 mL: 15-20 g; after the addition is completed, the system is placed at 30-40° C. and stirred for 40-60 min to obtain a sodium hydroxide solution.
[0013] Furthermore, the isopropanol aqueous solution is prepared by the following steps: adding isopropanol to deionized water with stirring, wherein the volume ratio of deionized water to isopropanol is 1:3-4; after the addition is completed, placing the system at 30-40° C. and stirring for 40-60 minutes to obtain the isopropanol aqueous solution.
[0014] Furthermore, the sodium chloroacetate-isopropanol aqueous solution is prepared by the following steps: adding isopropanol and sodium chloroacetate into deionized water with stirring, wherein the amount ratio of deionized water, isopropanol and sodium chloroacetate is 100mL:35g:5g, and the system is placed at 70-80°C and stirred for 40-60min to obtain the sodium chloroacetate-isopropanol aqueous solution.
[0015] Furthermore, a self-pumping bionic fiber membrane is used in an antibacterial dressing.
[0016] Beneficial effects of the present invention: The present invention provides a method for preparing a self-pumping bionic fiber membrane, wherein the electrospinning precursor liquid is stretched into nanofibers and collected on a modified non-woven fabric with excellent hydrophilic properties, thereby preparing a self-pumping bionic fiber membrane. The fiber membrane prepared by the present invention includes a double-layer structure, namely a non-woven fabric layer and a nanofiber layer, wherein the modified non-woven fabric layer is a hydrophilic liquid-absorbing layer, and the nanofiber layer is a hydrophobic drainage layer, which can achieve unidirectional liquid discharge. The present invention applies the self-pumping bionic fiber membrane prepared above to the field of dressings, specifically, to the healing of diabetic wounds, and can achieve unidirectional exudate directional drainage, thereby absorbing wound exudate, enriching coagulation substances, achieving coagulation, and promoting diabetic wound healing. The specific principles are as follows: First, the present invention prepares a modified non-woven fabric by modifying a PP non-woven fabric. Specifically, the present invention modifies the non-woven fabric into a highly liquid-absorbent non-woven fabric with a gelled surface through an alkalization reaction and an etherification reaction. The fiber surface of the modified non-woven fabric is gelled into carboxymethyl cellulose, which has excellent liquid absorption and moisture retention, while the fiber interior of the modified non-woven fabric is not gelled, providing ideal mechanical properties.
[0017] Then, the present invention selects bio-based polyamide as a hydrophobic drainage layer, and hydrophobically modifies the bio-based polyamide by using a hydrophobically modified slurry to obtain an electrospinning precursor solution, and then forms a hydrophobic drainage layer on the surface of the modified non-woven fabric through electrospinning, wherein the bio-based polyamide selected by the present invention is a bio-based PA11 material, and the bio-based PA11 material is made of 100% bio-based castor oil, which is safer and more environmentally friendly. The present invention then utilizes the excellent hydrophobicity of the fluorinated silane solution in the hydrophobically modified slurry to modify the bio-based PA11 material, and then forms a hydrophobic drainage layer on the surface of the modified non-woven fabric after electrospinning, and at the same time, the hydrophobic drainage layer has a fine and uniform microporous structure, which can become a one-way drainage channel for the liquid, and further realizes one-way liquid discharge.
[0018] Finally, the imidazole ring structure of the silane side chain in the fluorinated silane solution in the hydrophobically modified slurry prepared by the present invention has excellent antibacterial properties, which helps to improve the antibacterial effect of the self-pumping bionic fiber membrane. The prepared self-pumping bionic fiber membrane is then applied to the field of dressings to improve the antibacterial properties of the dressings. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0020] Example 1
[0021] A method for preparing a self-pumping bionic fiber membrane comprises the following steps: Step S1, preparing a modified solution: (1) Sodium hydroxide solution: Sodium hydroxide (AR; ≥96.0%; purchased from Sinopharm Chemical Reagent Co., Ltd.) was added to deionized water, wherein the ratio of deionized water to sodium hydroxide was 100 mL:15. After the addition was completed, the system was stirred at 30° C. for 40 min to obtain a sodium hydroxide solution.
[0022] (2) Isopropanol aqueous solution: isopropanol (AR; ≥99.7%; purchased from Sinopharm Chemical Reagent Co., Ltd.) was added to deionized water with stirring, wherein the volume ratio of deionized water to isopropanol was 1:3. After the addition was completed, the system was placed at 30° C. and stirred for 40 min to obtain an isopropanol aqueous solution.
[0023] (3) Sodium chloroacetate-isopropanol aqueous solution: isopropanol (AR; ≥99.7%; purchased from Sinopharm Chemical Reagent Co., Ltd.) and sodium chloroacetate (98%; purchased from Sinopharm Chemical Reagent Co., Ltd.) were added to deionized water with stirring, wherein the amount ratio of deionized water, isopropanol and sodium chloroacetate was 100 mL:35 g:5 g. The system was stirred at 70° C. for 40 min to obtain a sodium chloroacetate-isopropanol aqueous solution.
[0024] Step S2, preparing modified non-woven fabric: Select a weight of 15g / m 2 The PP non-woven fabric is immersed in the sodium hydroxide solution prepared in step S1, and alkalized at 35° C. for 30 minutes. After the alkalization is completed, an alkalized non-woven fabric is obtained. The alkalized non-woven fabric is then immersed in the sodium chloroacetate-isopropanol aqueous solution prepared in step S1, and etherified at 70° C. for 30 minutes. After the etherification is completed, an etherified non-woven fabric is obtained. The etherified non-woven fabric is then immersed in the isopropanol aqueous solution prepared in step S1, and a phosphoric acid aqueous solution with a mass fraction of 85% is added dropwise thereto to adjust the pH of the system to 6.5. After the pH adjustment is completed, the neutralized non-woven fabric is stirred at a constant temperature for 30 minutes to obtain a neutralized non-woven fabric, and the neutralized non-woven fabric is then rinsed with an isopropanol aqueous solution and deionized water for 3 times in sequence, and then dried at 120° C. for 30 minutes, taken out, and cooled to room temperature to obtain a modified non-woven fabric with excellent hydrophilic properties.
[0025] Step S3: Preparation of electrospinning precursor solution: 5-Difluoromethoxy-2-mercapto-1H-benzimidazole (99%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) was added to anhydrous ethanol (AR; ≥99.7%; purchased from Sinopharm Chemical Reagent Co., Ltd.) and stirred to dissolve. Dichloromethane (AR; ≥99.5%; purchased from Sinopharm Chemical Reagent Co., Ltd.) and vinyltrimethoxysilane (98%; purchased from Sinopharm Chemical Reagent Co., Ltd.) were then added. After the addition was completed, the mixture was stirred for 30 minutes, and then the initiator 2,2-dimethoxyphenylacetophenone (99%; purchased from Sinopharm Chemical Reagent Co., Ltd.) and the catalyst triethylenetetramine (CP) were added. ; purchased from Sinopharm Chemical Reagent Co., Ltd.), reacted for 20 minutes under 30W ultraviolet light irradiation to obtain a fluorinated silane solution, and then polypropylene (melt index 0.5g / 10min; purchased from Sinopharm Chemical Reagent Co., Ltd.) was added to the fluorinated silane solution, and stirred at high speed for 25 minutes to obtain a hydrophobic modified slurry, wherein the amount ratio of anhydrous ethanol, 5-difluoromethoxy-2-mercapto-1H-benzimidazole, dichloromethane, vinyltrimethoxysilane, 2,2-dimethoxyphenylacetophenone, triethylenetetramine and polypropylene is 40mL:0.22g:60mL:11.5mL:0.02g:0.01g:3.1g.
[0026] Bio-based polyamide (Agimid@PA11 bio-based polyamide from Arkema, France) was placed in a vacuum oven at 50°C for drying pretreatment for 5 hours, taken out and cooled to room temperature to obtain pretreated bio-based polyamide, and the pretreated bio-based polyamide was added and stirred into m-cresol (>99.0%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), and stirred for 2 hours at 35°C, and then the hydrophobically modified slurry was added and stirred at room temperature for 20 minutes to obtain an electrospinning precursor solution, wherein the amount ratio of m-cresol, pretreated bio-based polyamide and hydrophobically modified slurry was 10mL:4g:12mL.
[0027] Step S4: Preparation of self-pump biomimetic fiber membrane by electrospinning: The electrospinning precursor solution was stretched into nanofibers by an electrospinning machine and collected on the modified non-woven fabric. The electrospinning process parameters were as follows: the spinning box temperature was 22 °C, the relative humidity of the spinning box was 30%, the injection speed was 1.5 mL / h, the voltage was 18 kV, the electrospinning time was 5 h, the electrospinning collection distance was 15 cm, and the effective electrospinning area on the modified non-woven fabric was controlled at 300 cm. 2 After the electrospinning is completed, a self-pumping bionic fiber membrane is obtained.
[0028] Example 2
[0029] A method for preparing a self-pumping bionic fiber membrane comprises the following steps: Step S1, preparing a modified solution: (1) Sodium hydroxide solution: Sodium hydroxide (AR; ≥96.0%; purchased from Sinopharm Chemical Reagent Co., Ltd.) was added to deionized water, wherein the ratio of deionized water to sodium hydroxide was 100 mL:18 g. After the addition was completed, the system was stirred at 35° C. for 60 min to obtain a sodium hydroxide solution.
[0030] (2) Isopropanol aqueous solution: isopropanol (AR; ≥99.7%; purchased from Sinopharm Chemical Reagent Co., Ltd.) was added to deionized water with stirring, wherein the volume ratio of deionized water to isopropanol was 1:4. After the addition was completed, the system was placed at 40° C. and stirred for 60 min to obtain an isopropanol aqueous solution.
[0031] (3) Sodium chloroacetate-isopropanol aqueous solution: isopropanol (AR; ≥99.7%; purchased from Sinopharm Chemical Reagent Co., Ltd.) and sodium chloroacetate (98%; purchased from Sinopharm Chemical Reagent Co., Ltd.) were added to deionized water with stirring, wherein the amount ratio of deionized water, isopropanol and sodium chloroacetate was 100 mL:35 g:5 g. The system was stirred at 75 °C for 60 min to obtain a sodium chloroacetate-isopropanol aqueous solution.
[0032] Step S2, preparing modified non-woven fabric: Select the weight as 20g / m 2 The PP non-woven fabric is immersed in the sodium hydroxide solution prepared in step S1, and alkalized at 40° C. for 40 minutes. After the alkalization is completed, an alkalized non-woven fabric is obtained. The alkalized non-woven fabric is then immersed in the sodium chloroacetate-isopropanol aqueous solution prepared in step S1, and etherified at 75° C. for 40 minutes. After the etherification is completed, an etherified non-woven fabric is obtained. The etherified non-woven fabric is then immersed in the isopropanol aqueous solution prepared in step S1, and a phosphoric acid aqueous solution with a mass fraction of 85% is added dropwise thereto to adjust the pH of the system to 7.0. After the pH adjustment is completed, the neutralized non-woven fabric is stirred at a constant temperature for 40 minutes to obtain a neutralized non-woven fabric, and the neutralized non-woven fabric is then rinsed with an isopropanol aqueous solution and deionized water for 3 times in sequence, and then dried at 130° C. for 40 minutes, taken out, and cooled to room temperature to obtain a modified non-woven fabric with excellent hydrophilic properties.
[0033] Step S3: Preparation of electrospinning precursor solution: 5-Difluoromethoxy-2-mercapto-1H-benzimidazole (99%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) was added to anhydrous ethanol (AR; ≥99.7%; purchased from Sinopharm Chemical Reagent Co., Ltd.) and stirred to dissolve. Dichloromethane (AR; ≥99.5%; purchased from Sinopharm Chemical Reagent Co., Ltd.) and vinyltrimethoxysilane (98%; purchased from Sinopharm Chemical Reagent Co., Ltd.) were then added. After the addition was completed, the mixture was stirred for 40 minutes, and then the initiator 2,2-dimethoxyphenylacetophenone (99%; purchased from Sinopharm Chemical Reagent Co., Ltd.) and the catalyst triethylenetetramine (CP) were added. ; purchased from Sinopharm Chemical Reagent Co., Ltd.), reacted for 25 minutes under 30W ultraviolet light irradiation to obtain a fluorinated silane solution, and then polypropylene (melt index 0.5g / 10min; purchased from Sinopharm Chemical Reagent Co., Ltd.) was added to the fluorinated silane solution, and stirred at high speed for 30 minutes to obtain a hydrophobic modified slurry, wherein the amount ratio of anhydrous ethanol, 5-difluoromethoxy-2-mercapto-1H-benzimidazole, dichloromethane, vinyltrimethoxysilane, 2,2-dimethoxyphenylacetophenone, triethylenetetramine and polypropylene is 40mL:0.23g:60mL:11.8mL:0.02g:0.01g:3.2g.
[0034] Bio-based polyamide (Agimid@PA11 bio-based polyamide from Arkema, France) was placed in a vacuum oven at 55°C for drying pretreatment for 6 hours, taken out and cooled to room temperature to obtain pretreated bio-based polyamide, and the pretreated bio-based polyamide was added and stirred into m-cresol (>99.0%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), and stirred for 3 hours at 40°C, and then the hydrophobically modified slurry was added and stirred at room temperature for 30 minutes to obtain an electrospinning precursor solution, wherein the amount ratio of m-cresol, pretreated bio-based polyamide and hydrophobically modified slurry was 10mL:5g:14mL.
[0035] Step S4: Preparation of self-pump biomimetic fiber membrane by electrospinning: The electrospinning precursor liquid was stretched into nanofibers by an electrospinning machine and collected on the modified non-woven fabric. The electrospinning process parameters were as follows: the spinning box temperature was 25 °C, the relative humidity of the spinning box was 35%, the injection speed was 1.5 mL / h, the voltage was 18 kV, the electrospinning time was 5 h, the electrospinning collection distance was 15 cm, and the effective electrospinning area on the modified non-woven fabric was controlled at 300 cm 2 After the electrospinning is completed, a self-pumping bionic fiber membrane is obtained.
[0036] Example 3
[0037] A method for preparing a self-pumping bionic fiber membrane comprises the following steps: Step S1, preparing a modified solution: (1) Sodium hydroxide solution: Sodium hydroxide (AR; ≥96.0%; purchased from Sinopharm Chemical Reagent Co., Ltd.) was added to deionized water, wherein the amount ratio of deionized water to sodium hydroxide was 100 mL:20 g. After the addition was completed, the system was stirred at 40° C. for 60 min to obtain a sodium hydroxide solution.
[0038] (2) Isopropanol aqueous solution: isopropanol (AR; ≥99.7%; purchased from Sinopharm Chemical Reagent Co., Ltd.) was added to deionized water with stirring, wherein the volume ratio of deionized water to isopropanol was 1:4. After the addition was completed, the system was placed at 40° C. and stirred for 60 min to obtain an isopropanol aqueous solution.
[0039] (3) Sodium chloroacetate-isopropanol aqueous solution: isopropanol (AR; ≥99.7%; purchased from Sinopharm Chemical Reagent Co., Ltd.) and sodium chloroacetate (98%; purchased from Sinopharm Chemical Reagent Co., Ltd.) were added to deionized water with stirring, wherein the amount ratio of deionized water, isopropanol and sodium chloroacetate was 100 mL:35 g:5 g. The system was placed at 80° C. and stirred for 60 min to obtain a sodium chloroacetate-isopropanol aqueous solution.
[0040] Step S2, preparing modified non-woven fabric: Select a weight of 25g / m 2 The PP non-woven fabric is immersed in the sodium hydroxide solution prepared in step S1, and alkalized at 40° C. for 40 minutes. After the alkalization is completed, an alkalized non-woven fabric is obtained. The alkalized non-woven fabric is then immersed in the sodium chloroacetate-isopropanol aqueous solution prepared in step S1, and etherified at 80° C. for 40 minutes. After the etherification is completed, an etherified non-woven fabric is obtained. The etherified non-woven fabric is then immersed in the isopropanol aqueous solution prepared in step S1, and a phosphoric acid aqueous solution with a mass fraction of 85% is added dropwise thereto to adjust the pH of the system to 7.0. After the pH adjustment is completed, the neutralized non-woven fabric is stirred at a constant temperature for 40 minutes to obtain a neutralized non-woven fabric, and the neutralized non-woven fabric is then rinsed with an isopropanol aqueous solution and deionized water for 3 times in sequence, and then dried at 140° C. for 40 minutes, taken out, and cooled to room temperature to obtain a modified non-woven fabric with excellent hydrophilic properties.
[0041] Step S3: Preparation of electrospinning precursor solution: 5-Difluoromethoxy-2-mercapto-1H-benzimidazole (99%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) was added to anhydrous ethanol (AR; ≥99.7%; purchased from Sinopharm Chemical Reagent Co., Ltd.) and stirred to dissolve. Dichloromethane (AR; ≥99.5%; purchased from Sinopharm Chemical Reagent Co., Ltd.) and vinyltrimethoxysilane (98%; purchased from Sinopharm Chemical Reagent Co., Ltd.) were then added. After the addition was completed, the mixture was stirred for 40 minutes, and then the initiator 2,2-dimethoxyphenylacetophenone (99%; purchased from Sinopharm Chemical Reagent Co., Ltd.) and the catalyst triethylenetetramine (CP) were added. ; purchased from Sinopharm Chemical Reagent Co., Ltd.), reacted for 25 minutes under 30W ultraviolet light irradiation to obtain a fluorinated silane solution, and then polypropylene (melt index 0.5g / 10min; purchased from Sinopharm Chemical Reagent Co., Ltd.) was added to the fluorinated silane solution, and stirred at high speed for 30 minutes to obtain a hydrophobic modified slurry, wherein the amount ratio of anhydrous ethanol, 5-difluoromethoxy-2-mercapto-1H-benzimidazole, dichloromethane, vinyltrimethoxysilane, 2,2-dimethoxyphenylacetophenone, triethylenetetramine and polypropylene is 40mL:0.23g:60mL:12.0mL:0.02g:0.01g:3.2g.
[0042] Bio-based polyamide (Agimid@PA11 bio-based polyamide from Arkema, France) was placed in a vacuum oven at 60°C for drying pretreatment for 6 hours, taken out and cooled to room temperature to obtain pretreated bio-based polyamide, and the pretreated bio-based polyamide was added and stirred into m-cresol (>99.0%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), and stirred for 3 hours at 40°C, and then the hydrophobically modified slurry was added and stirred at room temperature for 30 minutes to obtain an electrospinning precursor solution, wherein the amount ratio of m-cresol, pretreated bio-based polyamide and hydrophobically modified slurry was 10mL:5g:15mL.
[0043] Step S4: Preparation of self-pump biomimetic fiber membrane by electrospinning: The electrospinning precursor solution was stretched into nanofibers by an electrospinning machine and collected on the modified non-woven fabric. The electrospinning process parameters were as follows: the spinning box temperature was 28 °C, the relative humidity of the spinning box was 40%, the injection speed was 1.5 mL / h, the voltage was 18 kV, the electrospinning time was 5 h, the electrospinning collection distance was 15 cm, and the effective electrospinning area on the modified non-woven fabric was controlled at 300 cm 2 After the electrospinning is completed, a self-pumping bionic fiber membrane is obtained.
[0044] Comparative Example 1 Comparative Example 1 is the control group of Example 2, in which the modification process of the nonwoven fabric in Example 2 is removed, that is, the electrospinning precursor solution is stretched into nanofibers by an electrospinning machine and collected on a plate having a gram weight of 20 g / m 2 The remaining raw materials, raw material amounts and preparation steps were kept the same as those in Example 2, and finally a self-pumping bionic fiber membrane was obtained.
[0045] Comparative Example 2 Comparative Example 2 is the control group of Example 2, in which the hydrophobically modified slurry in the preparation process of the electrospinning precursor solution in Example 2 is deleted, and the remaining raw materials, raw material amounts and preparation steps are kept the same as in Example 2, and finally a self-pumping bionic fiber membrane is obtained.
[0046] Specifically, the preparation process of the electrospinning precursor solution in Comparative Example 2 is as follows: the bio-based polyamide (Agimid@PA11 bio-based polyamide from Arkema, France) is placed in a vacuum oven at 55°C for drying pretreatment for 6 hours, taken out and cooled to room temperature to obtain pretreated bio-based polyamide, and the pretreated bio-based polyamide is added to m-cresol (>99.0%; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) with stirring, and the mixture is placed at 40°C and stirred for 3 hours to obtain an electrospinning precursor solution, wherein the amount ratio of m-cresol, pretreated bio-based polyamide and hydrophobically modified slurry is 10mL:5g.
[0047] Comparative Example 3 Comparative Example 3 is the control group of Example 2, except that the raw material 5-difluoromethoxy-2-mercapto-1H-benzimidazole in Example 2 is deleted, and the remaining raw materials, raw material amounts and preparation steps are kept the same as in Example 2, and finally a self-pumping bionic fiber membrane is obtained.
[0048] Test Example 1 The self-pumping bionic fiber membranes prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to performance tests. The performance test process is as follows, and the test results are shown in Table 1: Liquid absorption rate: Determine the liquid absorption rate of the self-pump bionic fiber membrane modified non-woven fabric layer (hydrophilic liquid absorption layer). The specific steps are as follows: Use an electronic balance to weigh 20×20mm 2 The self-pumping bionic fiber membrane was weighed and the dry weight was recorded as W1. It was then placed in a culture dish filled with 10 mL of deionized water and allowed to absorb liquid for 10 min at room temperature. It was then clamped with tweezers for 30 s to remove excess deionized water on the surface of the self-pumping bionic fiber membrane. The membrane was then reweighed and the wet weight was recorded as W2. The above steps were repeated 3 times, and the average liquid absorption rate was calculated, where the liquid absorption rate was calculated according to the following formula: Liquid absorption rate (%) = (W2-W1) / W1×100%.
[0049] Contact angle: The dynamic apparent contact angle of the self-pumping dressing was tested by dropping 5 μL of water on the self-pumping bionic fiber membrane nanofiber layer (hydrophobic drainage layer) using a contact angle tester.
[0050] Pore size determination: The gas permeation bubble point method was used to determine the pore size of the self-pump bionic fiber membrane nanofiber layer (hydrophobic drainage layer).
[0051] Antibacterial rate: The self-pump bionic fiber membranes prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were used as dressings, and the outer layer (nanofiber layer) of the dressings was subjected to an in vitro antibacterial test. The experimental process was as follows: 0.1 g of the nanofiber layer was taken and 10 mL of 1×10 7 The mixture of Escherichia coli liquid and Staphylococcus aureus liquid was placed in a test tube and placed on a constant temperature shaker at 37°C and 120 r / min for 4 h. This was used as the experimental group, and the one without the nanofiber layer was used as the blank group. The bacterial liquid of the experimental group and the blank group was taken out and diluted to 1×10 5 CFU / mL, 100 μL of bacterial solution was spread on the surface of the agar plate, and incubated in an oscillating incubator at 37°C and natural light conditions for 24 hours. The antibacterial rate was calculated by the plate colony counting method: Antibacterial rate (%) = (N a -N b )×100% / N a ; Among them, N a is the colony count of the blank group; N b is the colony number of the experimental group.
[0052] Among them, 1×10 7 The CFU / mL Escherichia coli solution / Staphylococcus aureus solution were obtained by culturing Escherichia coli (product number: TS337391; purchased from Ningbo Testo Biotechnology Co., Ltd.) and Staphylococcus aureus (product number: TS278079; purchased from Ningbo Testo Biotechnology Co., Ltd.) in the laboratory, respectively.
[0053] Table 1 Performance test results project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Liquid absorption rate / % 1250 1500 1650 450 1450 1450 Pore size / μm 0.14 0.13 0.14 0.13 0.13 0.13 Contact angle / ° 111.4 117.8 115.5 117.4 96.8 99.3 Antibacterial rate (Escherichia coli) / % 98.5 99.1 98.8 99.0 53.4 60.7 Antibacterial rate (Staphylococcus aureus) / % 97.3 98.0 97.6 97.8 50.1 54.5 The following conclusions can be drawn from Table 1: (1) Comparative Example 1 is the control group of Example 2. Compared with Example 2, Comparative Example 1 removes the modification process of the non-woven fabric layer (the fiber membrane includes a non-woven fabric layer and a nanofiber layer), that is, the process of modifying the non-woven fabric into a highly liquid-absorbent non-woven fabric with surface gelation by alkalization reaction and etherification reaction is removed. It can be seen from the data in Table 1 that the modification process significantly improves the liquid absorption performance of the non-woven fabric layer.
[0054] (2) Comparative Example 2 is the control group of Example 2. Compared with Example 2, Comparative Example 2 removes the hydrophobic modified slurry in the nanofiber layer (the fiber membrane includes a non-woven fabric layer and a nanofiber layer). It can be seen from the data in Table 1 that the addition of the hydrophobic modified slurry significantly improves the hydrophobicity and antibacterial (Escherichia coli + Staphylococcus aureus) properties of the nanofiber layer.
[0055] (1) Comparative Example 3 is the control group of Example 2. Compared with Example 2, Comparative Example 3 removes the raw material 5-difluoromethoxy-2-mercapto-1H-benzimidazole in the electrospinning precursor solution. It can be seen from the data in Table 1 that the addition of 5-difluoromethoxy-2-mercapto-1H-benzimidazole helps to improve the hydrophobicity and antibacterial (Escherichia coli + Staphylococcus aureus) properties of the nanofiber layer.
[0056] (4) From the data of Examples 1 to 3, it can be seen that the modified non-woven fabric layer of the self-pumping bionic fiber membrane prepared by the pre-protected embodiment scheme group of the present invention has excellent hydrophilic liquid absorption, and the nanofiber layer has excellent hydrophobicity, which can realize unidirectional liquid discharge, that is, realize "self-pumping". Furthermore, the self-pumping bionic fiber membrane prepared by Examples 1 to 3 of the present invention has excellent antibacterial (Escherichia coli + Staphylococcus aureus) performance.
[0057] It should be noted that, in this article, terms such as "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or equipment that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment.
[0058] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a self-pumping bionic fiber membrane, characterized in that: The following steps are involved: The bio-based polyamide is dried and pretreated, and the pretreated bio-based polyamide is added to the meta-cresol with stirring, and then stirred at 35-40°C for 2-3 hours, and then the hydrophobic modified slurry is added thereto with stirring, and stirred at room temperature for 20-30 minutes to obtain an electrospinning precursor solution, and the electrospinning precursor solution is stretched into nanofibers and collected on a modified non-woven fabric. After completion, a self-pumping bionic fiber membrane is obtained.
2. The method for preparing a self-pumping bionic fiber membrane according to claim 1, characterized in that: The dosage ratio of the meta-cresol, the pretreated bio-based polyamide and the hydrophobically modified slurry is 10 mL: 4-5 g: 12-15 mL.
3. The method for preparing a self-pumping bionic fiber membrane according to claim 1, characterized in that: The hydrophobically modified slurry is prepared by the following steps: Add 5-difluoromethoxy-2-mercapto-1H-benzimidazole to anhydrous ethanol, stir to dissolve, then add dichloromethane and vinyltrimethoxysilane, stir and mix for 30 to 40 minutes after the addition, then add 2,2-dimethoxyphenylacetophenone and triethylenetetramine, react under 30W ultraviolet light for 20 to 25 minutes to obtain a fluorine-containing silane solution, then add polypropylene to the fluorine-containing silane solution, stir at high speed for 25 to 30 minutes to obtain a hydrophobically modified slurry.
4. The method for preparing a self-pumping bionic fiber membrane according to claim 3, characterized in that: The dosage ratio of the anhydrous ethanol, 5-difluoromethoxy-2-mercapto-1H-benzimidazole, dichloromethane, vinyltrimethoxysilane, 2,2-dimethoxyphenylacetophenone, triethylenetetramine and polypropylene is 40mL: 0.22-0.23g: 60mL: 11.5-12.0mL: 0.02g: 0.01g: 3.1-3.2g.
5. The method for preparing a self-pumping bionic fiber membrane according to claim 1, characterized in that: The electrospinning process parameters are as follows: the spinning box temperature is 22-28°C, the relative humidity of the spinning box is 30%-40%, the injection speed is 1.5 mL / h, the voltage is 18 kV, the electrospinning time is 5 h, the electrospinning collection distance is 15 cm, and the effective electrospinning area on the modified nonwoven fabric is controlled at 300 cm 2 .
6. The method for preparing a self-pumping bionic fiber membrane according to claim 1, characterized in that: The modified nonwoven fabric is prepared by the following steps: The PP non-woven fabric was immersed in a sodium hydroxide solution and placed at 35 to 40°C for alkalization for 30 to 40 minutes. After completion, an alkalized non-woven fabric was obtained. The alkalized non-woven fabric was then immersed in a sodium chloroacetate-isopropanol aqueous solution and placed at 70 to 80°C for etherification for 30 to 40 minutes. After completion, an etherified non-woven fabric was obtained. The etherified non-woven fabric was then immersed in an isopropanol aqueous solution, and a phosphoric acid aqueous solution with a mass fraction of 85% was added dropwise to adjust the pH of the system to 6.5 to 7.
0. After completion, the neutralized non-woven fabric was obtained by constant temperature stirring for 30 to 40 minutes. The neutralized non-woven fabric was then rinsed three times with an isopropanol aqueous solution and deionized water, and then dried for 30 to 40 minutes, taken out, and cooled to room temperature to obtain a modified non-woven fabric.
7. The method for preparing a self-pumping bionic fiber membrane according to claim 6, characterized in that: The sodium hydroxide solution is prepared by the following steps: adding sodium hydroxide to deionized water, wherein the amount ratio of deionized water to sodium hydroxide is 100 mL: 15-20 g; after the addition is completed, placing the system at 30-40° C. and stirring for 40-60 minutes to obtain the sodium hydroxide solution.
8. The method for preparing a self-pumping bionic fiber membrane according to claim 6, characterized in that: The isopropanol aqueous solution is prepared by the following steps: adding isopropanol to deionized water with stirring, wherein the volume ratio of deionized water to isopropanol is 1:3-4; after the addition is completed, placing the system at 30-40° C. and stirring for 40-60 minutes to obtain the isopropanol aqueous solution.
9. The method for preparing a self-pumping bionic fiber membrane according to claim 6, characterized in that: The sodium chloroacetate-isopropanol aqueous solution is prepared by the following steps: adding isopropanol and sodium chloroacetate to deionized water with stirring, wherein the amount ratio of deionized water, isopropanol and sodium chloroacetate is 100 mL:35 g:5 g, and placing the system at 70-80° C. and stirring for 40-60 min to obtain the sodium chloroacetate-isopropanol aqueous solution.
10. Application of a self-pumping bionic fiber membrane in an antibacterial dressing, characterized in that: Use of the fiber membrane prepared by the preparation method according to any one of claims 1 to 9 in antibacterial dressings.
Citation Information
Patent Citations
Hydrophilic hydrophobic composite wound dressing for directing biological fluid and preparation method and application thereof
CN108175573A
Non-toxic environment-friendly solvent type double-layer nanofiber skin dressing and preparation method thereof
CN110772661A
Towel with cool and refreshing functions and preparation method thereof
CN111823672A
Preparation method of gelation modified fiber electrostatic spinning mask
CN113679618A
Far infrared healing-promoting electrostatic spinning wound dressing and preparation method thereof