Preparation method of flexible temperature-sensitive material and flexible temperature-sensitive material
Through electrospinning preparation and preoxidation carbonization treatment of C-SiC-Al2O3 composite material, Schottky-like diode structure is formed, which solves the problem of insufficient flexibility and accuracy of existing temperature sensors, and achieves high sensitivity and wide range Temperature sensing performance, simple process and low cost.
Patent Information
- Application Number
- CN202411096573.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-26
AI Technical Summary
Existing temperature sensors have shortcomings in flexibility, accuracy and biocompatibility, making them difficult to operate flexibly on curved surfaces and do not have high sensitivity temperature measurement capabilities.
Using C-SiC-Al2O3 composite material, nano-film materials are prepared through electrospinning technology, and Schottky-like diode structure is formed through preoxidation and carbonization treatment, combining the band conduction level characteristics of carbon-based fibers and graphene to form flexibility Temperature sensitive material.
It achieves temperature sensing performance with high sensitivity, wide working range and good environmental stability, and is simple in preparation process and low in cost, with good repeatability and temperature linear characteristics.
Smart Images

Figure CN119020888A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of semiconductor sensor materials, and more particularly, relates to a wide range of flexible temperature sensitive materials. Background Art
[0002] Temperature is one of the most commonly perceived factors in nature, as well as in humans and animals, and is also a basic function required by an electronic skin. This is mainly because temperature plays a vital role in daily life or in practical applications. Human body temperature plays an important role in monitoring human activities and determining human health status. Human body temperature is one of the important signals, which is closely related to the physiological and cognitive state of the human body. By monitoring human body temperature, very useful research value can be provided in the medical field, such as providing early warning for diseases related to body temperature changes (such as heat stroke, infection, fever, congestive heart failure, etc.). Due to its broad application prospects in the fields of human activity monitoring and personal health care, the development of electronic skin temperature sensing function has attracted more attention from researchers in recent years.
[0003] Resistive temperature detectors are one of the most widely used detectors, with the characteristics of fast response speed, high accuracy and high stability. In addition, thermal sensors, infrared temperature sensors and mercury thermometers are also widely used. In addition, the main materials of these sensors are ceramics, metals and metal oxides. However, some of their own characteristics limit them, including their inflexibility, large size and fragility, as well as the difficulty of attaching them to the curved surface of the object being measured. In many application scenarios, it is necessary to measure highly accurate temperature while taking into account easy operation, convenience, flexibility, softness and biocompatibility, which poses a very critical challenge to the research and preparation of flexible temperature sensors. Summary of the invention
[0004] In view of the shortcomings of the prior art or the need for improvement, the present invention provides a wide range of flexible temperature sensitive materials, which have high temperature sensitivity, good flexibility, a wide working range and good environmental stability.
[0005] The present invention provides a wide range of flexible temperature sensitive materials, including the following production steps:
[0006] Preparation of precursor solution: 1.2 g of polymer compound polyacrylonitrile (PAN) and 0.05 g of silicic acid powder (H2SiO3) were dissolved in 8.8 g of N,N-dimethylformamide (DMF), and stirred in a water bath magnetic stirrer at 60°C and 150 r / min for 6 h to fully dissolve PAN and silicic acid powder until a precursor solution was obtained.
[0007] Preparation of spinning solution: Weigh 0.3 g of aluminum chloride (AlCl3) and add it to the precursor solution, then stir it in a water bath magnetic stirrer at 60°C and 150 r / min for 8 h. After stirring evenly, let it stand for 24 h to degas, and obtain a spinning solution.
[0008] Electrospinning: The electrospinning device consists of an electrostatic high-voltage power supply, a syringe pump, and a roller collector. The roller diameter is 5 cm, the roller speed is set to 120 rad / min, the distance from the needle to the roller is fixed at 18 cm, the spinning solution feeding rate is 0.5 mL / h, and the voltage applied to the needle is 15 kV. After electrospinning, a nanofilm material is obtained.
[0009] Pre-oxidation: Set the temperature of the air circulation oven to 60℃ and the time to 3h for preliminary oxidation, and the nano film material will appear light yellow. Then set the temperature of the air circulation oven to 200℃ and the time to 2h for further oxidation, and the material will appear khaki. Finally, wait for the material to cool down naturally to complete the pre-oxidation.
[0010] Carbonization: The carbonization process was carried out in a nitrogen atmosphere. The temperature of the tube furnace was set to 800°C, the heating rate was 5°C / min, and the high-temperature carbonization time was 2h to obtain a flexible temperature-sensitive material.
[0011] Electrodes are attached to the flexible temperature sensitive material to perform temperature testing.
[0012] The flexible temperature-sensitive material provided by the present invention is mainly a C-SiC-Al2O3 composite material. Al2O3 doped in SiC can be regarded as an N-type semiconductor, and the carbon-based fiber has properties similar to graphene, and its conduction band energy level is higher than that of N-type SiC. Therefore, the two contact to form a Schottky diode structure. In a constant current and effective temperature range, there is a linear relationship between the forward voltage drop and the temperature change, and it has temperature-sensitive characteristics. Since there are a large number of SiC-like Schottky diode structures inside the prepared sensing material, it has good temperature sensing performance. Since the SBD formed is small in size and the interface is tightly bonded, the ideal factor is large, thereby improving the sensitivity. The cross-connection of multiple nanofibers allows Schottky diodes to form series, parallel and bridge paths in the fiber, so that the sensitivity is further improved and the temperature-sensitive performance is further optimized.
[0013] The present invention has the following characteristics and advantages:
[0014] The overall preparation process is simple and low-cost, including solution preparation, electrospinning, pre-oxidation and carbonization.
[0015] Flexible temperature sensitive materials have high sensitivity, wide working range, good repeatability and environmental stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0017] Figure 1 A flexible display diagram of the flexible temperature-sensitive material prepared by the present invention;
[0018] Figure 2 This is a scanning electron microscope (SEM) photograph of the flexible temperature sensitive material prepared by the present invention;
[0019] Figure 3 Energy dispersive spectrometer (EDS) of the flexible temperature sensitive material prepared by the present invention;
[0020] Figure 4 X-ray photoelectron spectroscopy (XPS) of the flexible temperature sensitive material prepared by the present invention;
[0021] Figure 5 The Raman spectrum (Raman) of the flexible temperature sensitive material prepared by the present invention;
[0022] Figure 6 The temperature-resistance change rate curve of the flexible temperature sensitive material prepared by the present invention at -170 to 300°C;
[0023] Figure 7 The sensitivity curve of the flexible temperature sensitive material prepared by the present invention;
[0024] Figure 8 The IV characteristic curve of the flexible temperature sensitive material prepared by the present invention;
[0025] Fig. 9 Cyclic test of the flexible temperature sensitive material prepared by the present invention;
[0026] Fig.10 This is an environmental humidity test of the flexible temperature sensitive material prepared by the present invention. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0028] like Figures 1 to 10 As shown, the present invention provides a wide range of flexible temperature sensitive materials, including the following production steps:
[0029] Preparation of precursor solution: 1.2 g of polymer compound polyacrylonitrile (PAN) and 0.05 g of silicic acid powder (H2SiO3) were dissolved in 8.8 g of N,N-dimethylformamide (DMF), and stirred in a water bath magnetic stirrer at 60°C and 150 r / min for 6 h to fully dissolve PAN and silicic acid powder until a precursor solution was obtained.
[0030] Preparation of spinning solution: Weigh 0.3 g of aluminum chloride (AlCl3) and add it to the precursor solution, then stir it in a water bath magnetic stirrer at 60°C and 150 r / min for 8 h. After stirring evenly, let it stand for 24 h to degas, and obtain a spinning solution.
[0031] Electrospinning: The electrospinning device consists of an electrostatic high-voltage power supply, a syringe pump, and a roller collector. The roller diameter is 5 cm, the roller speed is set to 120 rad / min, the distance from the needle to the roller is fixed at 18 cm, the spinning solution feeding rate is 0.5 mL / h, and the voltage applied to the needle is 15 kV. After electrospinning, a nanofilm material is obtained.
[0032] Pre-oxidation: Set the temperature of the air circulation oven to 60℃ and the time to 3h for preliminary oxidation, and the nano film material will appear light yellow. Then set the temperature of the air circulation oven to 200℃ and the time to 2h for further oxidation, and the material will appear khaki. Finally, wait for the material to cool down naturally to complete the pre-oxidation.
[0033] Carbonization: The carbonization process was carried out in a nitrogen atmosphere. The temperature of the tube furnace was set to 800°C, the heating rate was 5°C / min, and the high-temperature carbonization time was 2h to obtain a flexible temperature-sensitive material.
[0034] A flexible temperature sensor is prepared by attaching electrodes to the flexible temperature sensitive material and performing a temperature test.
[0035] The flexible temperature sensor was placed in a refrigeration and heating test device for resistance collection, and the test temperature range was -170℃~300℃. As the temperature increased, the resistance gradually decreased, and the curve showed good linear characteristics.
[0036] The flexible temperature sensor was tested by IV at a temperature range of 20-60°C and a voltage between ±1V. Under the condition of 20-60°C, the IV characteristic curve had a good linear relationship.
[0037] Repeatability is an important indicator to measure the self-recovery ability of a sensor. For this purpose, the flexible temperature sensor was subjected to a cycle test at 20 to 60°C. The resistance decreased with increasing temperature, and the peak value remained almost unchanged, indicating that it has good repeatability.
[0038] The flexible temperature sensor was placed in a humidity testing device at room temperature for resistance collection. The test humidity range was 40% to 80%. Changes in humidity had little effect on the resistance change rate, indicating that it is not humidity sensitive and has good environmental stability.
[0039] The flexible temperature-sensitive material provided by the present invention is mainly a C-SiC-Al2O3 composite material. Al2O3 doped in SiC can be regarded as an N-type semiconductor, and the carbon-based fiber has properties similar to graphene, and its conduction band energy level is higher than that of N-type SiC. Therefore, the two contact to form a Schottky diode structure. In a constant current and effective temperature range, there is a linear relationship between the forward voltage drop and the temperature change, and it has temperature-sensitive characteristics. Since there are a large number of SiC-like Schottky diode structures inside the prepared sensing material, it has good temperature sensing performance. Since the SBD formed is small in size and the interface is tightly bonded, the ideal factor is large, thereby improving the sensitivity. The cross-connection of multiple nanofibers allows Schottky diodes to form series, parallel and bridge paths in the fiber, so that the sensitivity is further improved and the temperature-sensitive performance is further optimized.
[0040] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for preparing a flexible temperature-sensitive material, characterized in that: The flexible temperature sensitive material comprises the following preparation steps: (1) Electrospinning: polyacrylonitrile (PAN) is dissolved in N,N-dimethylformamide (DMF), heated and stirred to obtain a precursor solution, silicon source and aluminum source are introduced, heated and stirred to obtain a spinning solution, and then the spinning solution is subjected to electrospinning to obtain a nanofilm material; (2) Heat treatment: The nano-film material is pre-oxidized and carbonized at high temperature to obtain a flexible temperature-sensitive material.
2. The method for preparing a flexible temperature sensitive material according to claim 1, characterized in that: In step (1), during the solution preparation process, polyacrylonitrile (PAN) is dissolved in N,N-dimethylformamide (DMF) to obtain a precursor solution, the silicon source is selected from silicic acid powder (H2SiO3), and the aluminum source is selected from aluminum chloride (AlCl3).
3. The method for preparing the flexible temperature sensitive material according to claim 2, characterized in that: During the solution preparation process, the precursor solution selects the polymer compound polyacrylonitrile (PAN) with a molecular weight of 15,000, the solvent selects the organic compound solvent N, N-dimethylformamide (DMF), and the mass ratio of solute to solvent is 1:6 to 1:
8.
4. The method for preparing a flexible temperature sensitive material according to claim 1, characterized in that: In the pre-oxidation treatment described in step (2), the atmosphere is controlled to be air, the initial temperature is set to 60° C. for 3 hours, and the secondary pre-oxidation temperature is set to 180-200° C. for 2 hours.
5. The method for preparing a flexible temperature sensitive material according to claim 1, characterized in that: In the high-temperature carbonization treatment described in step (2), the atmosphere is controlled to be nitrogen, the heating rate is 5°C / min, the temperature is 800°C, and the high-temperature carbonization time is 2h to obtain a flexible temperature-sensitive material.
6. A flexible temperature-sensitive material prepared by the method for preparing a flexible temperature-sensitive material as claimed in any one of claims 1 to 5, wherein the average fiber diameter is 360 nm, the average broken fiber rate is 2.9%, the uniformity coefficient is 0.25%, and the number of beads is 4.0 per 100 fibers.
7. The flexible temperature sensitive material according to claim 6, characterized in that: The material was cut into pieces with a length of 2 cm and a width of 1 cm, and then the electrodes were packaged for temperature testing.
8. The flexible temperature sensitive material according to claim 6, characterized in that: The flexible temperature sensitive material provided by the present invention is mainly a C-SiC-Al2O3 composite material. Al2O3 doped in SiC can be regarded as an N-type semiconductor, and the carbon-based fiber has properties similar to those of graphene, and its conduction band energy level is higher than that of N-type SiC. Therefore, the two are in contact to form a Schottky diode-like structure. In a constant current and effective temperature range, there is a linear relationship between the forward voltage drop and the temperature change, and the material has a temperature-sensitive characteristic. Since a large number of SiC-like Schottky diode structures exist inside the prepared sensing material, the material has good temperature sensing performance. Since the formed SBD is small in size and the interface is tightly bonded, the ideal factor is large, thereby improving the sensitivity. The cross-connection of multiple nanofibers allows the Schottky diodes to form series, parallel and bridge paths in the fibers, thereby further improving the sensitivity and optimizing the temperature-sensitive performance.
Citation Information
Cited By
Decoupling design of high-sensitivity flexible temperature-pressure dual-function sensor and preparation method of high-sensitivity flexible temperature-pressure dual-function sensor
CN119958756A