Sweat-absorbing and moisture-removing cloth and preparation method thereof
By using a combination of a thin intermediate layer and a composite layer of diatomaceous earth in sweat-absorbing and moisture-absorbing fabric, the problem of diatomaceous earth being easily blocked and not being combined for a long time in the footwear and clothing materials is solved, achieving long-lasting moisture absorption and breathability and good performance. Adhesion improves washing resistance.
Patent Information
- Application Number
- CN202411198085.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-26
AI Technical Summary
There are two major problems in the application of existing diatomaceous earth in footwear and clothing materials: one is that it is easy to be blocked by polymers, affecting moisture absorption and breathability; the other is that it does not combine with the fabric for a long time, has poor washing resistance, and does not work for a long time.
Use sweat-absorbent and wet-exhaust fabric composed of a fabric layer, an intermediate layer and a diatomaceous earth composite layer. The intermediate layer is made of an aqueous slurry by screen printing, including acrylic resin and polyurethane resin, and the diatomaceous earth composite layer contains a second acrylic resin The weight ratio of aqueous dispersion and diatomaceous earth is 3-5:10-15. The thinning of the intermediate layer increases the binding force and avoids polymer blockage.
The durable effect of diatomaceous earth is achieved, good moisture absorption and breathability are maintained, and the adhesion between the fabric and the diatomaceous earth composite layer is improved, which basically does not affect the feel of the fabric, and the washing resistance is improved through the optimization process.
Smart Images

Figure CN119021009A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textiles and relates to a sweat-absorbing and moisture-discharging fabric and a preparation method thereof. Background Art
[0002] Diatomaceous earth is a natural porous material with good adsorption and moisture absorption and breathability. It is widely used in shoes and clothing, giving shoes and clothing good moisture absorption and breathability and improving wearing comfort. There are two main application methods for diatomaceous earth in shoes and clothing materials: ① Disperse diatomaceous earth in polymers and prepare them into fibers, or first prepare them into diatomaceous earth masterbatch and then prepare them into fibers; ② Adsorb diatomaceous earth to the surface of fibers, fabrics, etc. by chemical adsorption or physical adsorption. In the above-mentioned first method, diatomaceous earth is not easy to separate from the fiber, has good washability and long action time, but the porous structure of diatomaceous earth is easily blocked by polymers, affecting its moisture absorption and breathability; in the second method, the porous structure of diatomaceous earth is well maintained, and the moisture absorption and breathability are good, but it is easy to fall off, has poor washability, and does not last long.
[0003] Therefore, the industry is in urgent need of a diatomaceous earth cloth that has both good moisture absorption and breathability and durability. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a sweat absorbing and moisture dissipating fabric and a preparation method thereof.
[0005] The technical solution of the present invention is as follows:
[0006] A sweat-absorbing and moisture-discharging fabric, comprising, from bottom to top, a fabric layer, an intermediate layer and a diatomaceous earth composite layer;
[0007] The thickness of the intermediate layer is 8-200 μm;
[0008] The thickness of the diatomite composite layer is 10-300 μm. The raw material components of the diatomite composite layer include a second acrylic resin aqueous dispersion and diatomite. The weight ratio of the second acrylic resin aqueous dispersion to the diatomite is 3-5:10-15.
[0009] Preferably, the intermediate layer is obtained from a first aqueous slurry by screen printing, and the raw material components of the first aqueous slurry include a first acrylic resin aqueous dispersion and a polyurethane aqueous dispersion.
[0010] More preferably, the weight ratio of the first acrylic resin aqueous dispersion to the polyurethane aqueous dispersion is 8-10:1-3.
[0011] More preferably, the first acrylic resin aqueous dispersion and the second acrylic resin aqueous dispersion are respectively selected from modified acrylic resin aqueous dispersions.
[0012] Further preferably, the modified acrylic resin aqueous dispersion is selected from one or a combination of two or more of epoxy modified acrylic resin aqueous dispersion, silicone modified acrylic resin aqueous dispersion and polyurethane modified acrylic resin aqueous dispersion.
[0013] More preferably, the polyurethane aqueous dispersion is selected from modified polyurethane dispersions.
[0014] Further preferably, the modified polyurethane dispersion is selected from one or a combination of two or more of silicone-modified polyurethane dispersion, epoxy-modified polyurethane dispersion and acrylic-modified polyurethane dispersion.
[0015] A method for preparing the sweat-absorbing and moisture-wicking fabric according to any of the above embodiments, comprising: applying a first aqueous slurry to one surface of the fabric by screen printing, applying a second aqueous slurry on the first aqueous slurry layer, and drying to obtain the fabric;
[0016] Alternatively, continue the above steps on the other side of the fabric.
[0017] Preferably, the raw material components of the first aqueous slurry include 8-10% by weight of the first acrylic resin aqueous dispersion and 1-3% by weight of the polyurethane aqueous dispersion of the first aqueous slurry.
[0018] Preferably, the raw material components of the second aqueous slurry include 3-5% by weight of the second acrylic resin aqueous dispersion and 10-15% by weight of the diatomaceous earth.
[0019] The beneficial effects of the present invention are:
[0020] (1) In order to solve the problem that diatomaceous earth is easily blocked by polymer, the present invention adds diatomaceous earth to an aqueous slurry, and the content of polymer in the aqueous slurry is very low, thereby weakening or even avoiding the blockage of the polymer on the porous structure of diatomaceous earth; in order to solve the problem that diatomaceous earth and fabric cannot be bonded for a long time, the present invention sets a very thin intermediate layer between the fabric and the diatomaceous earth composite layer, thereby improving the bonding force between the fabric and the diatomaceous earth composite layer, so that the effect of diatomaceous earth can be long-lasting and basically does not affect the feel of the fabric.
[0021] (2) The main resin of the aqueous slurry used in the middle layer of the present invention is a combination of acrylic resin and polyurethane resin, which not only maintains the good feel of the fabric but also has good bonding properties, making the effect of diatomaceous earth lasting.
[0022] (3) The sweat-absorbing and moisture-discharging fabric of the present invention can be printed with diatomaceous earth on one side or on both sides, which is flexible and convenient to operate. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Attached Figure 1 Schematic diagram of the structure of the sweat absorbing and moisture dissipating fabric according to Example 1 of the present invention. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is further illustrated and described below through specific implementation methods.
[0025] In order to solve the problem that the existing sweat-absorbing and moisture-wicking fabric using diatomaceous earth cannot achieve both durability and breathability, the present invention provides a sweat-absorbing and moisture-wicking fabric, which comprises, from bottom to top, a fabric layer (1), an intermediate layer (2) and a diatomaceous earth composite layer (3);
[0026] The thickness of the middle layer (2) is 8-200 μm;
[0027] The thickness of the diatomite composite layer (3) is 10-300 μm. The raw material components of the diatomite composite layer (3) include a second acrylic resin aqueous dispersion and diatomite. The weight ratio of the second acrylic resin aqueous dispersion to the diatomite is 3-5:10-15.
[0028] The present invention arranges diatomaceous earth on the surface of the fabric, and arranges an intermediate layer (2) between the fabric layer (1) and the diatomaceous earth composite layer (3), thereby improving the bonding force between the fabric layer (1) and the diatomaceous earth composite layer (3), and using less acrylic resin in the diatomaceous earth composite layer (3), thereby weakening or avoiding the blockage of the diatomaceous earth porous structure by the polymer, so that the sweat-absorbing and moisture-discharging fabric of the present invention has good air permeability and sweat-absorbing and moisture-discharging performance. In addition, the thickness of the intermediate layer (2) and the diatomaceous earth composite layer (3) is very thin, which basically does not affect the feel of the fabric.
[0029] In the present invention, the particle size of diatomaceous earth is not particularly limited, and the average particle size can be 1-20 μm. The thickness of the diatomaceous earth composite layer (3) is not less than the average particle size of the diatomaceous earth. For example, the thickness of the diatomaceous earth composite layer can be any value of 10 μm, 30 μm, 50 μm, 60 μm, 70 μm, 8 μm, 90 μm, 100 μm, 120 μm, 150 μm, 180 μm, 200 μm, 220 μm, 250 μm, 280 μm, 300 μm, etc., without special restrictions. Or, further, the thickness of the diatomaceous earth composite layer can be 10-100 μm. The weight ratio of the second acrylic resin aqueous dispersion and diatomaceous earth can be any value of 3:10, 3:12, 3:15, 4:10, 4:12, 4:15, 5:10, 5:12, etc., without special restrictions.
[0030] In a preferred embodiment of the present invention, the middle layer (2) is obtained by screen printing from the first aqueous slurry, and the raw material components of the first aqueous slurry include a first acrylic resin aqueous dispersion and a polyurethane aqueous dispersion. The middle layer (2) is obtained by screen printing, and the thickness can be relatively thin. Specifically, the thickness of the middle layer can be any value among 8μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, 75μm, 80μm, 85μm, 90μm, 95μm, 100μm, etc., without special restrictions. If the required thickness of the middle layer cannot be achieved by screen printing once, screen printing twice or three times can be used, and each screen printing can be directly operated on the previous screen printing, or can be operated after the previous screen printing is heated and cured. The raw material components of the first aqueous slurry include a first acrylic resin aqueous dispersion and a polyurethane aqueous dispersion, wherein the acrylic resin has good adhesion properties and the polyurethane can provide good hand feel and flexibility, so the middle layer takes into account adhesion, hand feel and flexibility, and has little influence on the hand feel of the fabric. The solid content of the above-mentioned polyurethane aqueous dispersion can be 15-50wt% (in the present invention, the test conditions for the solid content are 2g sample, baked at 120°C for 2h), such as any value of 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, etc., without special restrictions.
[0031] In a more preferred embodiment of the present invention, the weight ratio of the first acrylic resin aqueous dispersion and the polyurethane aqueous dispersion is 8-10:1-3. When the weight ratio of the first acrylic resin aqueous dispersion and the polyurethane aqueous dispersion is within the above range, the first aqueous slurry has a better effect, providing both better adhesion and better feel and flexibility. Specifically, the weight ratio of the first acrylic resin aqueous dispersion and the polyurethane aqueous dispersion can be any value of 8:1, 8:2, 8:3, 9:1, 9:2, 9:3, 10:1, 10:2, 10:3, etc., without special restrictions. In the present invention, the raw material components of the first aqueous slurry, in addition to the first acrylic resin aqueous dispersion and the polyurethane aqueous dispersion, may also include one or two or more of a leveling agent, a wetting agent, a defoamer, a thickener, a film-forming aid, an antioxidant, an anti-yellowing agent, etc., which are well known to those skilled in the art.
[0032] In a more preferred embodiment of the present invention, the first acrylic resin aqueous dispersion and the second acrylic resin aqueous dispersion are respectively selected from modified acrylic resin aqueous dispersions. The modified acrylic resin aqueous dispersion can have other properties in addition to the high adhesion of acrylic resin. For example, the modified acrylic resin aqueous dispersion can be selected from one or a combination of two or more of epoxy modified acrylic resin aqueous dispersion (with better adhesion and durability), silicone modified acrylic resin aqueous dispersion (with better high and low temperature resistance, weather resistance, flexibility, etc.) and polyurethane modified acrylic resin aqueous dispersion (with better flexibility, feel, etc.). The above-mentioned modified acrylic resin aqueous dispersions can be directly obtained on the market. In the present invention, the solid content of the first acrylic resin aqueous dispersion and the second acrylic resin aqueous dispersion can be 20-60wt%, such as any value of 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, etc., without special restrictions.
[0033] In a more preferred embodiment of the present invention, the polyurethane aqueous dispersion is selected from a modified polyurethane dispersion. The modified polyurethane dispersion may have other properties in addition to the properties of polyurethane. For example, the modified polyurethane dispersion may be selected from one or a combination of two or more of an organosilicon-modified polyurethane dispersion (having better high and low temperature resistance, weather resistance, flexibility, etc.), an epoxy-modified polyurethane dispersion (having better adhesion), and an acrylic acid-modified polyurethane dispersion (having higher strength, etc.).
[0034] On the other hand, the present invention provides a method for preparing the sweat-absorbing and moisture-wicking fabric described in any of the above embodiments, which can be obtained by a conventional screen printing method. Specifically, the steps may include: applying a first aqueous slurry to one side of the fabric by screen printing, and then applying a second aqueous slurry on the first aqueous slurry layer, and drying to obtain the fabric;
[0035] Alternatively, the above steps are continued on the other side of the fabric. Therefore, the fabric of the present invention can achieve the sweat absorption and moisture removal effect on one side or on both sides.
[0036] In a preferred embodiment of the present invention, the raw material components of the first aqueous slurry include 8-10% of the weight of the first aqueous slurry by weight of the first acrylic resin aqueous dispersion and 1-3% of the weight of the first aqueous slurry by weight of the polyurethane aqueous dispersion. In addition to the first acrylic resin aqueous dispersion and the polyurethane aqueous dispersion, the raw material components of the first aqueous slurry may also include a leveling agent, a wetting agent, a defoaming agent, a thickener, a film-forming aid, an antioxidant, an anti-yellowing agent, etc. The preparation method of the first aqueous slurry is well known to those skilled in the art.
[0037] In a preferred embodiment of the present invention, the raw material components of the second aqueous slurry include a second acrylic resin aqueous dispersion accounting for 3-5% of the weight of the second aqueous slurry and diatomaceous earth accounting for 10-15% of the weight of the second aqueous slurry. In the present invention, the raw material components of the second aqueous slurry, in addition to the second acrylic resin aqueous dispersion and diatomaceous earth, may also include one or two or more of a leveling agent, a wetting agent, a defoamer, a dispersant, a thickener, a film-forming aid, an antioxidant, an anti-yellowing agent, etc. The preparation method of the second aqueous slurry is well known to those skilled in the art.
[0038] The technical solution of the present invention is further described and illustrated according to various embodiments below. Unless otherwise specified, the parts described in the following embodiments are parts by weight.
[0039] First aqueous slurry:
[0040] The first aqueous slurry 1 is composed of: 8wt% aqueous epoxy-modified acrylic resin (solid content 40wt%), 1wt% aqueous polyurethane resin (solid content 30wt%), 88.6wt% water, 0.3wt% pH adjuster AMP-95, 0.3wt% dimethyl silicone defoamer, 1.2wt% polyurethane associative thickener, and 0.6wt% aqueous isocyanate curing agent.
[0041] The first aqueous slurry 2 is composed of: 10wt% aqueous acrylic resin (solid content 40wt%), 3wt% aqueous silicone modified polyurethane resin (solid content 30wt%), 84.8wt% water, 0.3wt% pH adjuster AMP-95, 0.3wt% dimethyl silicone defoamer, 1wt% polyurethane associative thickener, and 0.6wt% aqueous isocyanate curing agent.
[0042] The first aqueous slurry 3 is composed of: 13wt% aqueous acrylic resin (the aqueous acrylic resin in the first aqueous slurry 2), 84.8wt% water, 0.3wt% pH adjuster AMP-95, 0.3wt% dimethyl silicone defoamer, 1wt% polyurethane associative thickener, and 0.6wt% aqueous isocyanate curing agent.
[0043] The first aqueous slurry 4 is composed of: 13wt% aqueous silicone-modified polyurethane resin (the aqueous silicone-modified polyurethane resin in the first aqueous slurry 2), 84.8wt% water, 0.3wt% pH adjuster AMP-95, 0.3wt% dimethyl silicone defoamer, 1wt% polyurethane associative thickener, and 0.6wt% aqueous isocyanate curing agent.
[0044] Second aqueous slurry:
[0045] The second aqueous slurry 1 is composed of: 3wt% aqueous acrylic resin (solid content 40wt%), 84wt% water, 0.5wt% dispersant BYK190, 0.4wt% dimethyl silicone defoamer, 10wt% diatomaceous earth (average particle size 3μm), 1.3wt% hydroxyethyl cellulose ether, 0.5wt% pH adjuster AMP-95, and 0.3wt% aqueous isocyanate curing agent.
[0046] The second aqueous slurry 2 is composed of: 3wt% aqueous acrylic resin (the aqueous acrylic resin in the second aqueous slurry 1), 79wt% water, 0.5wt% dispersant BYK190, 0.4wt% dimethyl silicone defoaming agent, 15wt% diatomaceous earth (average particle size 3μm), 1.3wt% hydroxyethyl cellulose ether, 0.5wt% pH adjuster AMP-95, and 0.3wt% aqueous isocyanate curing agent.
[0047] The second aqueous slurry 3 is composed of: 3wt% aqueous acrylic resin (solid content 40wt%), 84wt% water, 0.5wt% dispersant BYK190, 0.4wt% dimethyl silicone defoamer, 10wt% diatomaceous earth (average particle size 10μm), 1.3wt% hydroxyethyl cellulose ether, 0.5wt% pH adjuster AMP-95, and 0.3wt% aqueous isocyanate curing agent.
[0048] The difference between the second aqueous slurry 4 and the second aqueous slurry 1 is that the aqueous acrylic resin is adjusted from 3 wt % to 10 wt %, and the water is adjusted from 84 wt % to 77 wt %. The other raw material compositions remain unchanged.
[0049] The difference between the second aqueous slurry 5 and the second aqueous slurry 1 is that the aqueous acrylic resin is adjusted from 3 wt % to 20 wt %, and the water is adjusted from 84 wt % to 67 wt %. The other raw material compositions remain unchanged.
[0050] Example 1
[0051] The first aqueous slurry 1 is screen-printed on one side of the fabric using a 300-mesh screen, with a film thickness of 25 μm. The second aqueous slurry 1 is screen-printed on the first aqueous slurry 1 film layer using a 200-mesh screen, with a film thickness of 30 μm. The film is transferred to an oven and baked at 60°C for 2 hours to obtain a sweat-absorbing and moisture-wicking fabric, the structure of which is shown in the attached figure. Figure 1 Indicates.
[0052] Example 2
[0053] The difference between this embodiment and embodiment 1 is that in embodiment 1, the second aqueous slurry 1 is replaced by the second aqueous slurry 2. The remaining steps remain unchanged.
[0054] Example 3
[0055] The difference between this embodiment and embodiment 1 is that in embodiment 1, the second aqueous slurry 1 is replaced by the second aqueous slurry 3. The other steps remain unchanged.
[0056] Example 4
[0057] The difference between this embodiment and embodiment 1 is that in embodiment 1, after screen printing the second aqueous slurry 1, another layer of the second aqueous slurry 1 is screen printed, and the total thickness of the second aqueous slurry layer 1 is 55 μm. The other steps remain unchanged.
[0058] Example 5
[0059] The difference between this embodiment and embodiment 1 is that in embodiment 1, after screen printing the second aqueous slurry 1, two more layers of the second aqueous slurry 1 are screen printed, and the total thickness of the second aqueous slurry layer 1 is 80 μm. The remaining steps remain unchanged.
[0060] Comparative Example 1
[0061] On one side of the fabric of Example 1, a second aqueous slurry 1 was screen-printed with a 200-mesh screen to a film thickness of 30 μm, and then transferred to an oven and baked at 60° C. for 2 hours to obtain a sweat-absorbing and moisture-wicking fabric.
[0062] Comparative Example 2
[0063] On one side of the fabric of Example 1, the first aqueous slurry 1 was screen-printed with a 300-mesh screen to a film thickness of 25 μm, and then transferred to an oven and baked at 60° C. for 2 hours to obtain a sweat-absorbing and moisture-wicking fabric.
[0064] Comparative Example 3
[0065] The difference between this comparative example and Example 1 is that in Example 1, the second aqueous slurry 1 is replaced by the second aqueous slurry 4. The other steps remain unchanged.
[0066] Comparative Example 4
[0067] The difference between this comparative example and Example 1 is that in Example 1, the second aqueous slurry 1 is replaced by the second aqueous slurry 5. The other steps remain unchanged.
[0068] Example 6
[0069] The first aqueous slurry 2 was screen-printed on one side of the cotton cloth using a 300-mesh screen, with a film thickness of 22 μm. The second aqueous slurry 2 was screen-printed on the first aqueous slurry 2 layer using a 250-mesh screen, with a film thickness of 35 μm. The mixture was then transferred to an oven and baked at 60° C. for 2 hours.
[0070] Example 7
[0071] The difference between this embodiment and embodiment 6 is that in embodiment 6, the first aqueous slurry 2 is replaced by the first aqueous slurry 3. The other steps remain unchanged.
[0072] Example 8
[0073] The difference between this embodiment and embodiment 6 is that in embodiment 6, the first aqueous slurry 2 is replaced by the first aqueous slurry 4. The remaining steps remain unchanged.
[0074] Example 9
[0075] The difference between this embodiment and embodiment 6 is that in embodiment 6, after baking, the first aqueous slurry 2 and the second aqueous slurry 2 are sequentially printed on the other side of the cotton cloth according to the steps of embodiment 6. The other steps remain unchanged.
[0076] The drying speed, water absorption rate and drip diffusion time were tested according to the method of GB / T 21655.1-2023. The results are shown in Table 1. The faster the drying speed, the higher the water absorption rate and the shorter the drip diffusion time, the better the moisture absorption and air permeability.
[0077] Adhesion test: Apply 3M 610 tape to the diatomaceous earth composite layer of the fabric without bubbles, load a 1Kg iron block on the tape, leave it for 30 seconds, remove the iron block and quickly tear off the tape to observe whether the coating is peeled off or damaged. Level 1: No damage or shedding at all; Level 2: <20% area damage or shedding; Level 3: 20-50% area damage or shedding; Level 4: Most of the damage or shedding; Level 5: Complete shedding.
[0078] Fabric feel: 10 trained volunteers will evaluate the score of the sweat-wicking fabric, with the feel of the untreated fabric being 1 point as the base score.
[0079] The results are shown in Table 1 below.
[0080] Table 1
[0081]
[0082] It can be seen from the data results in Table 1 above that the sweat-absorbing and moisture-discharging fabric of the present invention has excellent hydrophilicity, water absorption rate and drying speed, and has good sweat-absorbing and moisture-discharging performance. In addition, the diatomaceous earth composite layer has good adhesion to the fabric and basically does not affect the feel of the fabric.
[0083] After the sweat-absorbing and moisture-wicking fabric of the above-mentioned Example 1 was washed 5 times according to the standard washing method, the coating did not fall off or be damaged, the drying speed could reach 0.31 g / h, the water absorption rate could reach 103%, and the drip diffusion time could reach 2.4 s, indicating that the sweat-absorbing and moisture-wicking fabric of the present invention has good durability.
[0084] As described above, the basic principles, main features and advantages of the present invention are shown and described. Those skilled in the art should understand that the present invention is not limited by the above embodiments, which are only preferred embodiments of the present invention and cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the scope of the present invention and the content of the specification should still be within the scope of the present invention. The scope of protection required by the present invention is defined by the attached claims and their equivalents.
Claims
1. A sweat-absorbing and moisture-wicking fabric, characterized in that: From bottom to top, there are a fabric layer (1), an intermediate layer (2) and a diatomaceous earth composite layer (3); The thickness of the intermediate layer (2) is 8-200 μm; The thickness of the diatomite composite layer (3) is 10-300 μm. The raw material components of the diatomite composite layer (3) include a second acrylic resin aqueous dispersion and diatomite. The weight ratio of the second acrylic resin aqueous dispersion to the diatomite is 3-5:10-15.
2. The sweat wicking fabric according to claim 1, characterized in that: The intermediate layer (2) is obtained by screen printing from a first aqueous slurry, wherein the raw material components of the first aqueous slurry include a first acrylic resin aqueous dispersion and a polyurethane aqueous dispersion.
3. The sweat wicking fabric according to claim 2, characterized in that: The weight ratio of the first acrylic resin aqueous dispersion to the polyurethane aqueous dispersion is 8-10:1-3.
4. The sweat wicking fabric according to claim 2 or 3, characterized in that: The first acrylic resin aqueous dispersion and the second acrylic resin aqueous dispersion are respectively selected from modified acrylic resin aqueous dispersions.
5. The sweat wicking fabric according to claim 4, characterized in that: The modified acrylic resin aqueous dispersion is selected from one or a combination of two or more of epoxy modified acrylic resin aqueous dispersion, silicone modified acrylic resin aqueous dispersion and polyurethane modified acrylic resin aqueous dispersion.
6. The sweat wicking fabric according to claim 2 or 3, characterized in that: The polyurethane aqueous dispersion is selected from modified polyurethane dispersions.
7. The sweat wicking fabric according to claim 6, characterized in that: The modified polyurethane dispersion is selected from one or a combination of two or more of silicone-modified polyurethane dispersion, epoxy-modified polyurethane dispersion and acrylic acid-modified polyurethane dispersion.
8. A method for preparing the sweat absorbing and moisture dissipating fabric according to any one of claims 1 to 7, characterized in that: The steps include: Applying a first aqueous slurry to one side of the fabric by screen printing, applying a second aqueous slurry on the first aqueous slurry layer, and drying to obtain a fabric; Alternatively, continue the above steps on the other side of the fabric.
9. The method for preparing a sweat absorbing and moisture dissipating fabric according to claim 8, characterized in that: The raw material components of the first aqueous slurry include 8-10% of the first acrylic resin aqueous dispersion by weight of the first aqueous slurry and 1-3% of the polyurethane aqueous dispersion by weight of the first aqueous slurry.
10. The method for preparing a sweat absorbing and moisture dissipating fabric according to claim 8, characterized in that: The raw material components of the second aqueous slurry include 3-5% by weight of the second acrylic resin aqueous dispersion and 10-15% by weight of the diatomaceous earth.
Citation Information
Patent Citations
Environmental-friendly waterproof and breathable clothing leather and preparation method thereof
CN103835145A
Water-based hand feeling coating applied to automotive interiors and preparation method thereof
CN112552809A
Polyurethane synthetic leather with high moisture absorption and air permeability and preparation method thereof
CN113622201A
Water-based coating resin with high water resistance, moisture permeability and air permeability and preparation method thereof
CN115852710A
Moisture-conditioning wall material
JP2019196625A