Preparation method of composite material with porous coating and porous coating fabric

By adding water-absorbing resin particles to the surface of the textile and removing expanded particles to form a porous coating, the problem of difficulty in preparing a three-dimensional structure foam coating in the prior art is solved, and large-size bubble cells and uneven porous structures are realized, which improves the The breathability and aesthetics of the material.

CN119021017AActive Publication Date: 2024-11-26FUJIAN HUAFENG NEW MATERIALS
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411004190.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-26
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

In the prior art, methods for preparing foam coatings with three-dimensional structures on the surface of textiles are rarely disclosed. The existing foaming methods are mainly physical foaming and chemical foaming, making it difficult to form larger size bubble cells and uneven porous structures. .

Method used

A certain proportion of water-absorbent resin particles are added to the aqueous coating slurry, applied to the substrate surface and dried and soaked in water, so that the water-absorbent resin particles can be expanded and bubble cells are formed, and then the expanded resin particles are removed, and the particles of water-absorbent resin particles are adjusted by adjusting the particles of water-absorbent resin particles. The diameter, water absorption ratio and immersion time form a porous coating.

Benefits of technology

It is realized that bubble cells with 3D structure are formed on the surface of textiles, with a pore size of tens of μm to several millimeters, and the surface is uneven, which enhances breathability and aesthetics, and can adjust the size and shape of the holes according to parameters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119021017A_ABST
    Figure CN119021017A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a composite material with a porous coating and porous coating cloth, and relates to the technical field of porous composite materials. The preparation method of the composite material with the porous coating comprises the following steps: applying water-based coating slurry to the surface of a base material, drying for the first time, and soaking in water for a certain time to obtain a pre-expanded coating; the water-based coating slurry contains water-absorbent resin particles accounting for 1-25% of the weight of the water-based coating slurry; and removing the expanded water-absorbent resin particles in the pre-expanded coating, and drying for the second time to obtain the composite material with the porous coating. The composite materials with different bubble hole forms and sizes can be obtained through the simple preparation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of porous composite materials, and relates to a preparation method of a composite material with a porous coating and a porous coating cloth. Background Art

[0002] Coating a porous coating on the surface of textiles has many functions, including improving air permeability, aesthetics, heat insulation, etc. The existing porous coating is generally prepared by foaming, including physical foaming and chemical foaming. The pores are relatively fine and tiny, and the coating surface is relatively flat.

[0003] However, there are few methods disclosed in the prior art for preparing a foamed coating having a three-dimensional structure on the surface of a textile. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a composite material with a porous coating and a porous coating fabric.

[0005] The technical solution of the present invention is as follows:

[0006] A method for preparing a composite material having a porous coating, comprising:

[0007] Applying the aqueous coating slurry to the surface of the substrate, drying it for the first time, and then soaking it in water for a certain period of time to obtain a pre-expanded coating;

[0008] The aqueous coating slurry contains water-absorbing resin particles accounting for 1-25% of the weight of the aqueous coating slurry;

[0009] The expanded water-absorbing resin particles in the pre-expanded coating are removed, and the coating is dried for a second time to obtain the composite material having a porous coating.

[0010] Preferably, the aqueous coating slurry is one or a combination of two or more of aqueous PU slurry, aqueous modified PU slurry, aqueous acrylate slurry and aqueous modified acrylate slurry.

[0011] Preferably, the substrate has a porous structure.

[0012] More preferably, the substrate is a textile.

[0013] Preferably, the certain period of time is 10 minutes to 24 hours.

[0014] Preferably, the water absorption rate of the water-absorbing resin particles is 5-1000 times.

[0015] Preferably, the average particle size of the water-absorbing resin particles is 10 μm-5 mm.

[0016] Preferably, the removal is carried out by extrusion.

[0017] Preferably, the conditions for the first drying and the second drying are: temperature of 50-100° C., and time of 1-60 h, respectively.

[0018] A porous coated cloth is prepared by the method for preparing a composite material with a porous coating as described in any one of the above embodiments.

[0019] The beneficial effects of the present invention are:

[0020] (1) In the present invention, a certain proportion of water-absorbent resin particles are added to an aqueous coating slurry, which is then applied to the surface of a substrate and immersed in water after drying and curing. The water-absorbent resin particles absorb water and expand by a large multiple, and the coating undergoes obvious foaming, or further the outer surface of the coating can be broken. The resin particles that have absorbed water and expanded are removed, and a porous coating can be obtained.

[0021] (2) The present invention can obtain bubbles with a 3D structure, the surface of which can be uneven to form a concave-convex structure, and the size of the obtained bubble pores can be adjusted according to the particle size of the water-absorbing resin particles, the amount of water-absorbing resin particles added, and the water absorption rate.

[0022] (3) The present invention can obtain bubbles of larger size, and the size of the bubbles can reach 1 mm, or even more than 5 mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a photograph of the porous coated fabric of Example 1.

[0024] Figure 2 This is a photograph of the porous coated fabric of Example 2.

[0025] Figure 3 This is a photograph of the dried printing paint of Example 9.

[0026] Figure 4 This is a photograph of the porous coated cloth of Example 9. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is further illustrated and described below through specific implementation methods.

[0028] In one aspect, the present invention provides a method for preparing a composite material having a porous coating, comprising:

[0029] Applying the aqueous coating slurry to the surface of the substrate, drying it for the first time, and then soaking it in water for a certain period of time to obtain a pre-expanded coating;

[0030] The aqueous coating slurry contains water-absorbing resin particles accounting for 1-25% by weight of the aqueous coating slurry;

[0031] The expanded water-absorbing resin particles in the pre-expanded coating are removed and dried for a second time to obtain the composite material with a porous coating of the present invention.

[0032] The present invention introduces water-absorbent resin particles into the aqueous coating slurry. After the slurry is formed and solidified, it is immersed in water. The water-absorbent resin in the coating gradually absorbs water and expands a large multiple, foaming to form bubble holes, and even further bursting the coating. After the expanded water-absorbent resin is removed in a simple manner, bubble holes are formed at the expanded water-absorbent resin position. The size of the bubble hole can be adjusted according to the particle size of the water-absorbent resin particles, the amount of water-absorbent resin particles added, and the water absorption rate. The size of the bubble hole can be as low as tens of μm, or can reach mm level, or even larger.

[0033] The water-absorbent resin can absorb dozens to hundreds of times of its own water. In order to avoid the water-absorbent resin particles added to absorb a large amount of water in the water-based coating slurry, resulting in the water-based coating slurry viscosity is too large to be coated, the present invention can directly add the water-absorbent resin to the prepared water-based coating slurry, and stir and disperse for no more than 5min, or stir and disperse for no more than 3min, or stir and disperse for no more than 1min, the stirring and dispersing speed is not particularly limited, and can be 200-1500rpm, and then immediately applied to the surface of the substrate. In the present invention, the water-based coating slurry can be applied to the surface of the substrate by scraping, screen printing, etc., without special restrictions. The thickness of the applied slurry coating is not particularly limited, but generally greater than the average particle size of the water-absorbent resin particles, or can be 1.5 times or more of the average particle size of the water-absorbent resin particles, such as the average particle size of the water-absorbent resin particles is 0.5mm, the thickness of the slurry coating can be 1mm, 2mm, etc., such as the average particle size of the water-absorbent resin particles is 1mm, the thickness of the slurry coating can be 2mm, 3mm, 5mm, etc.

[0034] Regarding the weight proportion of the water-absorbent resin particles in the aqueous coating slurry, further, the weight proportion of the water-absorbent resin particles in the aqueous coating slurry can be 5-22%. For example, the weight proportion can be any value among 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, etc., but not limited to the above-listed ones.

[0035] In a preferred embodiment of the present invention, there is no particular limitation on the aqueous coating slurry, as long as it can form a film on the surface of the substrate and form good adhesion, it can be a single-component aqueous coating slurry or a two-component aqueous coating slurry. The components of the aqueous coating slurry except the water-absorbing resin particles can be called "aqueous slurry", which can be purchased directly from the market or prepared according to the method of the prior art. Specifically, the aqueous slurry can be one or a combination of two or more of aqueous PU slurry, aqueous modified PU slurry, aqueous acrylate slurry and aqueous modified acrylate slurry. For example, a kind of aqueous slurry, according to 100% by weight, the raw material composition can be as follows: 50-70wt% aqueous modified PU resin, 10-30wt% water, 0.3-0.6wt% defoamer, 0.5-2wt% thickener, 3-6wt% propylene glycol, 4-8wt% crosslinking agent (can be an aqueous polyisocyanate crosslinking agent).

[0036] In a preferred embodiment of the present invention, the substrate has a porous structure. The substrate has a porous structure, which can increase the permeability with the aqueous coating slurry and improve the adhesion, which is more conducive to the stability of the coating.

[0037] In a more preferred embodiment of the present invention, the substrate is a textile. The material of the textile in the present invention is not particularly limited, and can be a textile of natural material or a textile of artificial synthetic material. Natural materials include cotton, linen, wool, etc., and artificial synthetic materials include polyester, nylon, polypropylene, spandex, acrylic, chloroprene, etc., but are not limited to the above-mentioned ones. In the present invention, the textile can specifically be cloth, such as commonly used clothing cloth, curtain cloth, flame retardant cloth, fire resistant cloth, etc.

[0038] In a preferred embodiment of the present invention, the certain time is 10min-24h. By controlling the time when the coating is immersed in water, the water absorption and expansion ratio of the water-absorbing resin can be adjusted, and then the size of the bubble pores obtained or whether the bubble pores are broken can be adjusted. Further preferably, the certain time is 0.5h-12h, for example, it can be any value of 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, 10h, 10.5h, 11h, 11.5h, 12h, etc., but not limited to the above. Or, further, the certain time can be 1-8h.

[0039] In a preferred embodiment of the present invention, the water absorption rate of the water-absorbing resin particles is 5-1000 times. In the present invention, the water-absorbing resin particles can be cross-linked polyacrylic acid salts, starch acrylate polymers, starch-acrylonitrile graft copolymers, acrylamide-acrylonitrile-acrylic acid terpolymers, etc. The water absorption rate of the water-absorbing resin can be adjusted according to the different materials of the water-absorbing resin particles, the different cross-linking degrees, etc. Further preferably, the water absorption rate of the water-absorbing resin particles is 10-500 times. For example, the water absorption rate can be 10 times, 20 times, 30 times, 40 times, 50 times, 60 times, 70 times, 80 times, 90 times, 100 times, 110 times, 120 times, 130 times, 140 times, 150 times, 160 times, 170 times, 180 times, 190 times, 200 times, 220 times, 250 times, 280 times, 300 times, 320 times, 330 times, 350 times, 370 times, 400 times, 430 times, 450 times, 470 times, 500 times, etc., any value, but not limited to the above-listed ones.

[0040] In the present invention, the water absorption rate of the water-absorbing resin particles can be tested as follows: at 23° C., a certain weight W1 of dry water-absorbing resin is immersed in clean water for 24 hours, taken out, the moisture on the outer surface of the resin is removed, and the weight M2 is weighed, then, the water absorption rate = (M2-M1) / M1.

[0041] In a preferred embodiment of the present invention, the average particle size of the water-absorbing resin particles is 10 μm-5 mm. By adjusting the average particle size of the water-absorbing resin particles, the size of the obtained bubble pores can also be adjusted. From the dimension of the water-absorbing resin particles, the average particle size of the water-absorbing resin particles can further be 100 μm-5 mm. For example, the average particle size can be any value of 100 μm, 200 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, 4.5 mm, 5 mm, etc., but is not limited to the above-mentioned ones.

[0042] In a preferred embodiment of the present invention, the removal method is extrusion. Due to the high expansion ratio of the water-absorbing resin particles, the pore walls of the expanded coating pores become very thin, and the pore walls can be broken by a simple extrusion method, and the water-absorbing resin particles are squeezed out, thereby forming pores; when the expansion ratio of the water-absorbing resin particles is very high and the pores are broken, the water-absorbing resin particles can be separated from the composite material by turning over the composite material, thereby forming pores.

[0043] In a preferred embodiment of the present invention, the conditions for the first drying and the second drying are: temperature of 50-100°C and time of 1-60h. By heating and drying at a low temperature, the coating can achieve solidification and high adhesion on the substrate. For example, the first drying and the second drying can be 50°C × 6h, 60°C × 3h, 70°C × 12h, 60°C × 12h, 60°C × 24h, 60°C × 36h, 70°C × 24h, 80°C × 2h, 80°C × 6h, etc. In addition, from the purpose and effect of the first drying and the second drying, the temperature of the second drying can be higher or the time can be longer, so that the curing effect of the coating can be better, for example, the first drying can be 60°C × 12h, and the second drying can be 60°C × 36h or 70°C × 24h. Of course, during the first drying, since the slurry contains more water, it can be left at room temperature for a period of time to allow most of the water to evaporate, such as 1-12 hours, and then heated for drying, which is understandable to those skilled in the art.

[0044] On the other hand, the present invention provides a porous coated fabric, which is prepared by the method for preparing a composite material with a porous coating as described in any of the above embodiments. The porous coated fabric of the present invention has a base material of fabric, and because the fabric has a sparse expanded pore structure, the coating and the fabric can have a good bonding force, and a 3D cellular structure is formed on the fabric.

[0045] The technical solution of the present invention is further described and illustrated according to various embodiments below. Unless otherwise specified, the parts described in the following embodiments are parts by weight.

[0046] In the following embodiments and comparative examples of the present invention, the composition of the aqueous slurry is as follows: 65.7wt% aqueous acrylic modified PU resin, 22wt% water, 0.5wt% defoamer (dimethyl silicone oil), 0.8wt% thickener (associative polyurethane thickener), 5wt% propylene glycol, 6wt% crosslinker (aqueous polyisocyanate curing agent). The composition of the above aqueous slurry is only an example of the present invention, which is used to further illustrate the embodiments of the present invention and does not represent a limitation of the present invention. It can be understood by those skilled in the art that the aqueous slurries of the embodiments and comparative examples of the present invention can also be composed of other raw materials or directly obtained from the market.

[0047] The water-absorbing resin particles are cross-linked sodium acrylate particles.

[0048] Water-absorbent resin particles 1: average particle size 0.2 mm, water absorption rate 300 times;

[0049] Water-absorbent resin particles 2: average particle size 1 mm, water absorption rate 80 times;

[0050] Water-absorbing resin particles 3: average particle size 3 mm, water absorption rate 220 times.

[0051] Example 1

[0052] 5 parts of water-absorbing resin particles 1 were added to 95 parts of the stirred aqueous slurry, stirred at 800 rpm for 1 minute, and then printed on the cloth using a hollow one-layer screen to obtain a printed cloth. The printed cloth was placed at room temperature for 4 hours, then dried overnight at 60°C, placed at room temperature for 24 hours, then immersed in water at room temperature for 3 hours, taken out, and the expanded water-absorbing resin particles were removed from the printed coating by squeezing, and then continued to dry at 60°C for 36 hours, taken out and cooled to obtain a porous coated cloth.

[0053] A photo of the porous coated cloth of this embodiment is shown in the attached Figure 1 As shown, the coating has obvious air bubbles and is uneven, with a 3D effect, and the expanded air bubbles are less likely to be broken.

[0054] Example 2

[0055] The difference between Example 2 and Example 1 is that in Example 1, the water-absorbing resin particles 1 are adjusted from 5 parts to 22 parts, and the aqueous slurry is adjusted from 95 parts to 78 parts. The other steps remain unchanged.

[0056] A photo of the porous coated cloth of this embodiment is shown in the attached Figure 2 As shown, the coating has obvious air bubbles. Due to the high content of water-absorbing resin particles and the high water absorption expansion multiple, the expanded air bubbles are basically broken.

[0057] Comparative Example 1

[0058] The difference between Comparative Example 1 and Example 1 is that in Example 1, no water-absorbing resin particles are added, and the coating does not generate a porous structure or swell.

[0059] Example 3

[0060] 12 parts of water-absorbing resin particles 2 were added to 88 parts of the stirred aqueous slurry, stirred at 600 rpm for 1 minute, and then printed on the cloth using a hollow one-layer screen to obtain a printed cloth. The printed cloth was placed at room temperature for 1 hour, then at 60°C for 6 hours, and at room temperature for 24 hours, then immersed in water at room temperature for 1 hour, taken out, and the expanded water-absorbing resin particles were removed from the printed coating by squeezing, and then continued to dry at 60°C for 48 hours, taken out and cooled, to obtain a porous coated cloth.

[0061] The porous coated fabric of this embodiment has obvious air bubbles, and less than 10% of the air bubbles are broken.

[0062] Example 4

[0063] The difference between Example 4 and Example 3 is that in Example 3, the time for immersing the coating in water at room temperature after curing is increased from 1 hour to 2 hours. The other steps remain unchanged.

[0064] The porous coated fabric of this embodiment has obvious air bubbles, and the size of the air bubbles is obviously larger than that of the air bubbles in Embodiment 3, and almost 30% of the air bubbles are broken.

[0065] Example 5

[0066] The difference between Example 5 and Example 3 is that in Example 3, the time for immersing the coating in water at room temperature after curing is increased from 1 hour to 4 hours. The other steps remain unchanged.

[0067] The porous coated fabric of this embodiment has obvious air bubbles, and the size of the air bubbles is significantly larger than that of the air bubbles in Embodiment 4, and almost 80% of the air bubbles are broken.

[0068] Example 6

[0069] The difference between Example 6 and Example 3 is that in Example 3, the time for immersing the coating in water at room temperature after curing is increased from 1 hour to 10 hours. The other steps remain unchanged.

[0070] The porous coated fabric of this embodiment has obvious air bubbles, and the size of the air bubbles is close to that of the air bubbles in Embodiment 5, and more than 95% of the air bubbles are broken.

[0071] Example 7

[0072] The difference between Example 7 and Example 4 is that in Example 4, the water-absorbing resin particles 2 are replaced by water-absorbing resin particles 1 of equal weight. The other steps remain unchanged.

[0073] The porous coated fabric of this embodiment has obvious air bubbles, and the size of the air bubbles is significantly smaller than that of the air bubbles in Embodiment 4, and no more than 5% of the air bubbles are broken.

[0074] Example 8

[0075] The difference between Example 8 and Example 4 is that in Example 4, the water-absorbing resin particles 2 are replaced by water-absorbing resin particles 3 of equal weight. The other steps remain unchanged.

[0076] The porous coated fabric of this embodiment has obvious air bubbles, and the size of the air bubbles is significantly larger than that of the air bubbles in Embodiment 4, and more than 90% of the air bubbles are broken.

[0077] Example 9

[0078] 6 parts of water-absorbing resin particles (commercially available product Ocean Baby) were added to 94 parts of the stirred aqueous slurry, stirred at 800 rpm for 1 minute, and then printed on the cloth using a hollow one-layer screen printing plate to obtain a printed cloth. The printed cloth was placed at room temperature for 4 hours and then dried at 60°C overnight. The appearance was as shown in the attached figure. Figure 3 The dried printed fabric was placed at room temperature for 24 hours, then immersed in water at room temperature for 3 hours, taken out, and the expanded water-absorbing resin particles were removed from the printed coating by squeezing, and then dried at 60°C for 36 hours, taken out and cooled, to obtain a porous coated fabric with an appearance as shown in the attached figure. Figure 4 shown.

[0079] The above embodiments demonstrate that the composite material with a porous structure of the present invention can form an uneven porous structure on the surface of the substrate, and the shape and size of the porous structure can be adjusted by adjusting the amount of water-absorbing resin particles added, the particle size, the water absorption time, etc.

[0080] As described above, the basic principles, main features and advantages of the present invention are shown and described. Those skilled in the art should understand that the present invention is not limited by the above embodiments, which are only preferred embodiments of the present invention and cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the scope of the present invention and the content of the specification should still be within the scope of the present invention. The scope of protection required by the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a composite material having a porous coating, characterized in that: include: Applying the aqueous coating slurry to the surface of the substrate, drying it for the first time, and then soaking it in water for a certain period of time to obtain a pre-expanded coating; The aqueous coating slurry contains water-absorbing resin particles accounting for 1-25% of the weight of the aqueous coating slurry; The expanded water-absorbing resin particles in the pre-expanded coating are removed, and the coating is dried for a second time to obtain the composite material having a porous coating.

2. The method for preparing a composite material having a porous coating according to claim 1, characterized in that: The aqueous coating slurry is one or a combination of two or more of aqueous PU slurry, aqueous modified PU slurry, aqueous acrylate slurry and aqueous modified acrylate slurry.

3. The method for preparing a composite material having a porous coating according to claim 1, characterized in that: The substrate has a porous structure.

4. The method for preparing a composite material having a porous coating according to claim 3, characterized in that: The substrate is a textile.

5. The method for preparing a composite material having a porous coating according to claim 1, characterized in that: The certain time is 10min-24h.

6. The method for preparing a composite material having a porous coating according to claim 1, characterized in that: The water absorption rate of the water-absorbing resin particles is 5-1000 times.

7. The method for preparing a composite material having a porous coating according to claim 1, characterized in that: The average particle size of the water absorbing resin particles is 10 μm-5 mm.

8. The method for preparing a composite material having a porous coating according to claim 1, characterized in that: The removal method is extrusion.

9. The method for preparing a composite material having a porous coating according to claim 1, characterized in that: The conditions of the first drying and the second drying are respectively: temperature of 50-100° C. and time of 1-60 h.

10. A porous coated fabric, characterized in that: The composite material with a porous coating is prepared by the method for preparing the composite material with a porous coating according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Manufacturing method of polyacrylic acid-series water-absorbent resin

    CN108192013A

  • Water sucking resin microspheres for water-based coating and preparation method thereof

    CN109370294A

  • Self-foaming multi-functional water-based moisture absorption coating and preparation method thereof

    CN113717623A

  • Sound insulation coating and preparation method thereof

    CN117089269A

  • Porous formed product and manufacturing method for the same, hydrous water-absorbing polymer particle and manufacturing method for the same, method for adjusting water-absorbing rate of hydrous water-absorbing polymer particle, and porous sheathed electric wire