Preparation method of cotton stalk biochemical mechanical pulp

Through the two-stage enzyme treatment of cellulase and compound enzyme, combined with biological and chemical methods, the problems of low efficiency and unutilization of resources in cotton stalk pulping process are solved, the pulp quality and cotton stalk utilization rate are improved, and the The use and pollution of chemical drugs have achieved efficient pulp preparation and alleviated the shortage of paper-making raw materials.

CN119021027APending Publication Date: 2024-11-26QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)

Patent Information

Application Number
CN202411160323.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art has problems such as long processing time, low efficiency and high chemical consumption in cotton stew pulping process, which affects the quality and environment of pulping, and the cotton stew resources are not fully utilized.

Method used

Cellulase and compound enzyme are used to treat two stages of enzymes, hydrolyzing cotton stalk cellulose and degrading pectin in cotton stalk skin, improving the refining efficiency and pulp performance, combining biological methods and chemical methods to reduce the use of chemical drugs and pollution load.

Benefits of technology

It improves the utilization rate of cotton stalks, improves the quality of pulp, reduces the use and pollution of chemicals, realizes efficient pulp preparation, and alleviates the shortage of paper raw materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of cotton stalk biochemical mechanical pulp. The preparation method comprises the following steps: cutting cleaned and dried cotton stalks into sections, and then sequentially carrying out pre-steaming and spiral extrusion filament separation treatment; the cotton stalks subjected to thread rolling are soaked in a buffer solution of cellulase for enzyme treatment for set time, and then the cotton stalks are soaked in a hot alkali solution; sequentially carrying out high-concentration pulping and latency treatment on the cotton stalks subjected to the hot alkali dipping treatment, and carrying out two-stage enzyme treatment on the obtained crude pulp by adopting a compound enzyme of xylanase and pectinase; and performing pulp screening and PFI pulping on the pulp subjected to the two-stage enzyme treatment to obtain the cotton stalk biochemical mechanical pulp. Cellulase and compound enzyme are respectively used for carrying out two-stage enzyme treatment on cotton stalks, the treatment effect of chemicals is improved under the action of enzymes, the pulping efficiency is promoted, and the paper pulp performance is improved. The method can improve the utilization rate of the cotton stalks, turns waste into wealth, and effectively relieves the problem of shortage of papermaking raw materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pulping and papermaking, and in particular relates to a method for preparing cotton stalk biochemical mechanical pulp. Background Art

[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.

[0003] As the main byproduct of cotton, cotton stalks are mainly used for composting, fuel and livestock feeding, while the other part is directly burned or discarded in the field. The value of cotton stalks as biomass resources has not been fully utilized. Therefore, if cotton stalks are used in the pulp and paper industry, the use of cotton stalks, which are originally low-value agricultural waste, can not only bring certain economic value, but also alleviate the shortage of papermaking raw materials in my country. For cotton stalk raw materials, choosing appropriate pulping and papermaking methods to match the raw materials can produce paper and paperboard suitable for different purposes.

[0004] Pulping methods can significantly affect the quality of paper and are roughly divided into chemical and mechanical methods. The chemical method uses chemicals to treat plant fiber raw materials under specific conditions. This method has a lower pulp yield and a higher cellulose content. Mechanical pulping is a method that relies on mechanical action to achieve fiber separation. Using this method, most of the hemicellulose and lignin can be retained, the yield is high, and the pulp has long fibers. Biotechnology has attracted much attention due to its environmental friendliness and can be used to improve the properties of mechanical pulp from cotton stalks. There are two main types of biotechnology used in the pulping process, one is the use of fungi for pretreatment, and the other is the direct addition of bioenzymes during the pulping process. However, the use of fungal treatment in the pulping process has the disadvantages of long processing time and low efficiency. Therefore, bioenzymes are more suitable for pulping and papermaking processes due to their specificity, high efficiency and mild action conditions.

[0005] In addition to fiber cells, cotton stalks also contain a large number of miscellaneous cells, which will increase the consumption of liquid medicine during the pulping process and affect the final paper quality. In order to improve the quality of pulp and remove impurities, a large amount of chemicals are often required, which increases the cost and the load of wastewater treatment. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing biochemical mechanical pulp of cotton stalks. Cotton stalks are treated with cellulase and compound enzymes in two stages, and the effect of enzymes is used to improve the treatment effect of chemicals, promote pulping efficiency, and improve pulp performance. This method can improve the utilization rate of cotton stalks, turn waste into treasure, and effectively alleviate the problem of shortage of papermaking raw materials.

[0007] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0008] A method for preparing cotton stalk biochemical mechanical pulp comprises the following steps:

[0009] The cleaned and dried cotton stalks are cut into sections and then subjected to pre-steaming and spiral extrusion and filament separation processes in sequence;

[0010] The rolled cotton stalks are immersed in a buffer solution of cellulase for enzyme treatment for a set time, and then immersed in a hot alkaline solution;

[0011] After the hot alkali impregnated cotton stalks are subjected to high-concentration pulping and latent removal treatments in sequence, the obtained crude pulp is subjected to a two-stage enzyme treatment using a compound enzyme of xylanase and pectinase;

[0012] The pulp treated with the second-stage enzyme is subjected to screening and PFI beating to obtain the cotton stalk biochemical mechanical pulp.

[0013] In some embodiments, the length of the cotton stalks after cutting is 4-6 cm.

[0014] In some embodiments, the parameters of pre-steaming are: solid-liquid ratio of 1:4-8, g / mL; treatment temperature of 90-100° C.; and treatment time of 30-50 min. The pre-steaming in the present invention treats the cotton stalks with hot steam to improve the effect of cotton stalk extrusion and filament separation.

[0015] In some embodiments, the compression ratio of the spiral extrusion filament separation is 1:3-6, preferably 1:4. In the present invention, the spiral extrusion filament separation process of the cotton stalk can fully separate the raw materials, which is beneficial to subsequent processing.

[0016] In some embodiments, the buffer in the cellulase buffer solution is a citric acid-sodium citrate solution with a pH value of 4.5-6.5.

[0017] Preferably, the dosage of the cellulase is 5-15 U / g relative to the absolute dry material.

[0018] Preferably, when the rolled cotton stalks are immersed in a buffer solution of cellulase for enzyme treatment, the solid-liquid ratio is 1:4-6 g / mL, the treatment temperature is 45-55° C., and the treatment time is 30-90 min.

[0019] The invention adopts cellulase to treat cotton stalks, hydrolyzes part of amorphous cellulose in the cotton stalks, thereby improving the effect of subsequent hot alkali impregnation treatment.

[0020] In some embodiments, during the hot alkali impregnation treatment, the mass concentration of sodium hydroxide in the hot alkali is 2%-6%, preferably 3-5%.

[0021] Preferably, the temperature of the hot alkali immersion treatment is 90-100° C., and the time of the hot alkali immersion treatment is 30-50 min.

[0022] More preferably, the temperature of the hot alkali impregnation treatment is 92-97° C., and the time of the hot alkali impregnation treatment is 35-45 min.

[0023] Hot alkali impregnation of cotton stalks is an indispensable step in the preparation of chemical mechanical pulp.

[0024] In some embodiments, the rotation speed of the high-concentration refining is 3000-3500 rpm, and the refining is carried out in two stages. The gap of the first stage of refining is 0.3 mm, and the gap of the second stage of refining is 0.15 mm.

[0025] In some embodiments, in the compound enzyme, the enzymatic activity ratio of xylanase to pectinase is 1-2:1-2, and the total enzyme dosage of the compound enzyme is 25-35 U / g, relative to the absolute dry material.

[0026] Preferably, the total enzyme dosage of the compound enzyme is 27-33 U / g.

[0027] Preferably, the buffer solution of the composite enzyme is a citric acid-sodium citrate solution with a pH value of 4-6.

[0028] Preferably, the solid-liquid ratio for the second-stage enzyme treatment is 1:4-6 g / mL, the treatment temperature is 40-60° C., and the treatment time is 30-90 min.

[0029] In view of the chemical composition structure of the raw materials and the high pectin content of cotton stalk peel, xylanase and pectinase were selected to treat the pulp in a targeted manner to significantly improve the pulp quality.

[0030] In some embodiments, the PFI pulp has a freeness of 40±2° SR.

[0031] The beneficial effects achieved by one or more embodiments of the present invention are as follows:

[0032] (1) The present invention uses cotton stalks as raw materials and invents a method for preparing cotton stalk biochemical mechanical pulp. Cotton stalks are derived from cotton production and need urgent attention to be paid to fully utilize them. Using cotton stalks for pulping can not only alleviate the shortage of domestic papermaking raw materials, but also increase the utilization of cotton stalks and bring good economic value.

[0033] (2) The present invention proposes a two-stage enzyme treatment. The first stage of enzyme treatment uses cellulase to hydrolyze the amorphous area of ​​cotton stalk cellulose in a targeted manner, which can improve the accessibility of the liquid medicine in the subsequent treatment process, improve the pulping efficiency, and improve the quality of pulp; the second stage of enzyme treatment uses a composite enzyme, which is composed of xylanase and pectinase. Xylanase can promote the hydrolysis of hemicellulose, thereby promoting the removal of part of lignin and improving the effect of alkali impregnation and pulping. Pectinase can degrade pectin in cotton stalk skin to prevent it from becoming dissolved substances and colloidal substances, which have an adverse effect on the pulping quality and the bonding force between pulp fibers. The two enzymes can produce a synergistic effect and improve the quality of pulp more efficiently. The two-stage enzyme treatment has different effects, which can improve the effect of pulping, improve the performance of pulp, and make the pulp more in line with product requirements.

[0034] (3) The present invention adopts a processing method combining biological and chemical methods to invent a cotton stalk biochemical mechanical pulp based on the raw material characteristics of cotton stalks. The combination of biological and chemical methods in the preparation of cotton stalk mechanical pulp not only utilizes the high efficiency, specificity and mild action of biological enzymes, but also reduces the use of chemical drugs, saves energy consumption, reduces pollution load, and improves the performance of cotton stalk mechanical pulp in a targeted manner. DETAILED DESCRIPTION

[0035] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0036] The present invention will be further described below in conjunction with the embodiments.

[0037] The materials involved in the examples can be purchased from the market. All biological enzymes are from Shandong Longkote Enzyme Preparation Co., Ltd. The enzyme activity of xylanase is 50000 U / mL, the enzyme activity of pectinase is 90000 U / mL, and the enzyme activity of cellulase is 80000 U / mL.

[0038] The cotton stalks used in the following examples are from Dezhou, Shandong, with a cellulose content of 42.37%, hemicellulose of 17.41%, lignin of 21.87%, and ash of 2.06%.

[0039] Example 1

[0040] (1) Cut the washed and air-dried cotton stalks into segments with a length of 4 to 6 cm.

[0041] (2) The cotton stalks obtained in step (1) are subjected to pre-steaming treatment, wherein the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the treatment temperature is 95° C., and the treatment time is 40 min.

[0042] (3) The cotton stalks obtained in step (2) are subjected to a spiral extrusion process before cooling, and the compression ratio is 1:4.

[0043] (4) The cotton stalks obtained in step (3) are treated with enzymes in a buffer solution containing cellulase, wherein the cellulase activity is 5 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH value of 4.5, the solid-liquid ratio is 1:5 g / mL, the treatment temperature is 50°C, and the treatment time is 60 min.

[0044] (5) The cotton stalk obtained in step (4) is subjected to hot alkali immersion treatment in a hot alkali solution, the amount of sodium hydroxide used is 4%, the solid-liquid ratio of the immersion is 1:4 g / mL, the treatment temperature is 95° C., and the treatment time is 40 min.

[0045] (6) The cotton stalks obtained in step (5) are subjected to high-concentration grinding at a rotation speed of 3500 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, latent removal is performed.

[0046] (7) The slurry obtained in step (6) is subjected to a second-stage enzyme treatment in a buffer solution containing a composite enzyme, wherein the composite enzyme ratio (enzyme activity) used is xylanase: pectinase = 2:1, the total enzyme activity is 30 U / g, the buffer is a citric acid-sodium citrate solution with a pH value of 6.0, the solid-liquid ratio is 1:5 g / mL, the treatment temperature is 50°C, and the treatment time is 60 min.

[0047] (8) The pulp obtained in step (7) is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheets are made.

[0048] Results: The pulp yield was 76.89% and the tear index of the paper sheet was 6.22 mN·m 2 / g, the tensile index is 33.43N·m / g, and the ring compression index is 11.12N·m / g.

[0049] Example 2

[0050] The difference from Example 1 is step (4), and the remaining steps are the same as those of Example 1:

[0051] (4) The cotton stalks obtained in step (3) are treated with enzymes in a buffer solution containing cellulase, wherein the cellulase activity is 10 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH value of 6.0, the solid-liquid ratio is 1:6 g / mL, the treatment temperature is 55°C, and the treatment time is 75 min.

[0052] Results: The pulp yield was 76.54% and the tear index of the paper sheet was 6.09 mN·m 2 / g, the tensile index is 30.88N·m / g, and the ring compression index is 10.87N·m / g.

[0053] Example 3

[0054] The difference from Example 1 is step (4), and the remaining steps are the same as those of Example 1:

[0055] (4) The cotton stalks obtained in step (3) are treated with enzymes in a buffer solution containing cellulase, wherein the cellulase activity is 15 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH value of 5.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 45°C, and the treatment time is 30 min.

[0056] Results: The pulp yield was 77.24% and the tear index of the paper sheet was 6.19 mN·m 2 / g, the tensile index is 32.92N·m / g, and the ring compression index is 10.96N·m / g.

[0057] Example 4

[0058] The difference from Example 1 is step (7), and the remaining steps are the same as Example 1.

[0059] (7) The slurry obtained in step (6) is subjected to a two-stage enzyme treatment in a buffer solution containing a composite enzyme, wherein the composite enzyme ratio (enzyme activity) used is xylanase: pectinase = 1:2, the total enzyme activity is 30 U / g, the buffer is a citric acid-sodium citrate solution with a pH value of 5.0, the solid-liquid ratio is 1:6 g / mL, the treatment temperature is 55°C, and the treatment time is 90 min.

[0060] Results: The pulp yield was 77.04% and the tear index of the paper sheet was 6.14 mN·m 2 / g, the tensile index is 32.73N·m / g, and the ring compression index is 10.92N·m / g.

[0061] Example 5

[0062] The difference from Example 1 is step (7), and the remaining steps are the same as Example 1.

[0063] (7) The slurry obtained in step (6) is subjected to a second-stage enzyme treatment in a buffer solution containing a composite enzyme, wherein the composite enzyme ratio (enzyme activity) used is xylanase: pectinase = 1:1, the total enzyme activity is 30 U / g, the buffer is a citric acid-sodium citrate solution with a pH value of 4.5, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 45°C, and the treatment time is 45 min.

[0064] Results: The pulp yield was 77.04% and the tear index of the paper sheet was 6.06 mN·m 2 / g, the tensile index is 30.92N·m / g, and the ring compression index is 10.61N·m / g.

[0065] Example 6

[0066] The difference from Example 1 is step (7), and the remaining steps are the same as Example 5.

[0067] (7) The slurry obtained in step (6) is subjected to a second-stage enzyme treatment in a buffer solution containing a composite enzyme, wherein the composite enzyme ratio (enzyme activity) used is xylanase: pectinase = 1:1, the total enzyme activity is 30 U / g, the buffer is a citric acid-sodium citrate solution with a pH value of 6.0, the solid-liquid ratio is 1:5 g / mL, the treatment temperature is 50°C, and the treatment time is 90 min.

[0068] Results: The pulp yield was 77.01%, and the tear index of the paper sheet was 6.2 mN·m 2 / g, the tensile index is 32.98N·m / g, and the ring compression index is 11.04N·m / g.

[0069] Comparative Example 1

[0070] The difference from Example 1 is that cellulase is omitted in step (1), and xylanase and pectinase are omitted in step (7), as follows:

[0071] (4) The twisted cotton stalk obtained in step (3) is treated in a buffer solution, wherein the buffer solution is a citric acid-sodium citrate solution with a pH value of 4.5, a solid-liquid ratio of 1:5 g / mL, a treatment temperature of 50° C., and a treatment time of 60 min.

[0072] (7) The slurry obtained in step (6) is treated with a buffer solution, wherein the buffer solution is a citric acid-sodium citrate solution with a pH value of 4.5, a solid-liquid ratio of 1:4 g / mL, a treatment temperature of 45° C., and a treatment time of 45 min.

[0073] Results: The pulp yield was 81.17% and the tear index of the paper sheet was 5.47 mN·m 2 / g, the tensile index is 27.11N·m / g, and the ring compression index is 9.44N·m / g.

[0074] Comparative Example 2

[0075] The difference from Example 1 is step (7), and the remaining steps are the same as Example 1, which are as follows:

[0076] (7) The slurry obtained in step (6) is treated with a buffer solution, wherein the buffer solution is a citric acid-sodium citrate solution with a pH value of 4.5, a solid-liquid ratio of 1:4 g / mL, a treatment temperature of 45° C., and a treatment time of 45 min.

[0077] Results: The pulp yield was 79.65%, and the tear index of the paper sheet was 5.78 mN·m 2 / g, the tensile index is 29.65N·m / g, and the ring compression index is 9.97N·m / g.

[0078] Comparative Example 3

[0079] The difference from Example 5 is step (4), and the rest is the same as Example 5, which is as follows:

[0080] (4) The twisted cotton stalk obtained in step (3) is treated in a buffer solution, wherein the buffer solution is a citric acid-sodium citrate solution with a pH value of 4.5, a solid-liquid ratio of 1:5 g / mL, a treatment temperature of 50° C., and a treatment time of 60 min.

[0081] Results: The pulp yield was 80.78% and the tear index of the paper sheet was 5.93 mN·m 2 / g, the tensile index is 30.03N·m / g, and the ring compression index is 10.17N·m / g.

[0082] Comparative Example 4

[0083] The difference from Example 5 is Example (7), and the rest is the same as Example 1.

[0084] (7) The slurry obtained in step (6) is subjected to a second-stage enzyme treatment in a buffer solution containing xylanase, wherein the xylanase activity used is 20 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH value of 4.5, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 45° C., and the treatment time is 45 min.

[0085] Results: The pulp yield was 79.79% and the tear index of the paper sheet was 5.98 mN·m 2 / g, the tensile index is 30.65N·m / g, and the ring compression index is 10.37N·m / g.

[0086] Comparative Example 5

[0087] The difference from Example 5 is Example (7), and the rest is the same as Example 1.

[0088] (7) The slurry obtained in step (6) is subjected to a second-stage enzyme treatment in a buffer solution containing pectinase, wherein the pectinase activity used is 20 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH value of 4.5, the solid-liquid ratio is 1:4, the treatment temperature is 45° C., and the treatment time is 45 min.

[0089] Results: The pulp yield was 79.95%, and the tear index of the paper sheet was 5.88 mN·m 2 / g, the tensile index is 30.28N·m / g, and the ring compression index is 10.25N·m / g.

[0090] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing cotton stalk biochemical mechanical pulp, characterized in that: The steps include: The cleaned and dried cotton stalks are cut into sections and then subjected to pre-steaming and spiral extrusion and filament separation processes in sequence; The rolled cotton stalks are immersed in a buffer solution of cellulase for enzyme treatment for a set time, and then immersed in a hot alkaline solution; After the hot alkali impregnated cotton stalks are subjected to high-concentration pulping and latent removal treatments in sequence, the obtained crude pulp is subjected to a two-stage enzyme treatment using a compound enzyme of xylanase and pectinase; The pulp treated with the second-stage enzyme is subjected to screening and PFI beating to obtain the cotton stalk biochemical mechanical pulp.

2. The method for preparing cotton stalk biochemical mechanical pulp according to claim 1, characterized in that: The length of the cotton stalk after cutting is 4-6cm.

3. The method for preparing biochemical mechanical pulp of cotton stalks according to claim 1, characterized in that: The parameters of pre-steaming are: solid-liquid ratio is 1:4-8, g / mL; processing temperature is 90-100°C; processing time is 30-50min.

4. The method for preparing biochemical mechanical pulp of cotton stalks according to claim 1, characterized in that: The compression ratio of the spiral extrusion filament is 1:3-6, preferably 1:

4.

5. The method for preparing cotton stalk biochemical mechanical pulp according to claim 1, characterized in that: The buffer in the cellulase buffer solution is a citric acid-sodium citrate solution with a pH value of 4.5-6.5; Preferably, the amount of the cellulase is 5-15 U / g relative to the absolute dry material; Preferably, when the rolled cotton stalks are immersed in a buffer solution of cellulase for enzyme treatment, the solid-liquid ratio is 1:4-6 g / mL, the treatment temperature is 45-55° C., and the treatment time is 30-90 min.

6. The method for preparing biochemical mechanical pulp of cotton stalks according to claim 1, characterized in that: During the hot alkali impregnation treatment, the mass concentration of sodium hydroxide in the hot alkali is 2%-6%, preferably 3-5%; Preferably, the temperature of the hot alkali impregnation treatment is 90-100°C, and the time of the hot alkali impregnation treatment is 30-50 minutes; Preferably, the temperature of the hot alkali impregnation treatment is 92-97° C., and the time of the hot alkali impregnation treatment is 35-45 min.

7. The method for preparing cotton stalk biochemical mechanical pulp according to claim 1, characterized in that: The rotation speed of the high-concentration refining is 3000-3500 rpm, and the refining is carried out in two stages. The gap of the first stage refining is 0.3 mm, and the gap of the second stage refining is 0.15 mm.

8. The method for preparing biochemical mechanical pulp of cotton stalks according to claim 1, characterized in that: In the compound enzyme, the enzyme activity ratio of xylanase to pectinase is 1-2:1-2, and the total enzyme dosage of the compound enzyme is 25-35 U / g relative to the absolute dry material. Preferably, the total enzyme dosage of the compound enzyme is 27-33U / g; Preferably, the buffer solution of the composite enzyme is a citric acid-sodium citrate solution with a pH value of 4-6.

9. The method for preparing biochemical mechanical pulp of cotton stalks according to claim 8, characterized in that: The solid-liquid ratio for the second-stage enzyme treatment is 1:4-6 g / mL, the treatment temperature is 40-60°C, and the treatment time is 30-90 min.

10. The method for preparing biochemical mechanical pulp of cotton stalks according to claim 1, characterized in that: The beating degree of PFI pulping is 40±2°SR.

Citation Information

Patent Citations

  • Process for preparing pulp by using salix mongolia by chemical mechanical method

    CN102174760A

  • Method for improving drainability of cotton stalk chemi-mechanical pulp

    CN118147937A

Cited By

  • Enzymatic pulping process for improving performance of cultural paper and application of enzymatic pulping process

    CN119736809A

  • Energy-saving method for preparing high-yield pulp by taking wood and bamboo materials as raw materials through two-stage biological enzyme treatment

    CN121760232A

  • Method for preparing cotton-stalk biochemomechanical pulp

    WO2026040326A1