Optimized construction method for industrial factory building steel fiber reinforced concrete terrace
By optimizing the material specifications and construction process of steel fiber reinforced concrete, the cracking and settlement problems of steel fiber reinforced concrete flooring in industrial plants have been solved, achieving high-quality construction results and resource conservation.
Patent Information
- Application Number
- CN202411085903.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-26
AI Technical Summary
Existing steel fiber reinforced concrete flooring is prone to cracking, sanding, and uneven settlement under harsh operating conditions, failing to meet the high requirements of industrial plants.
By optimizing the specifications of steel fiber raw materials and concrete mix proportions, combined with plastic film laying, laser leveling and wear-resistant material treatment, the uniformity and strength of steel fiber concrete are ensured, and cracking and settlement are prevented.
It enables high-quality construction of steel fiber reinforced concrete flooring, prevents cracking and settlement, saves construction costs, promotes resource reuse, and improves construction efficiency and floor durability.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to a steel fiber concrete floor, and in particular to an optimized construction method for a steel fiber concrete floor of an industrial plant. Background Art
[0002] In recent years, with the rapid development of industries such as logistics, automobiles, medicine, and intelligent manufacturing, as well as the demand for industrial intelligence, customers have higher and higher requirements for the use of flooring, and pay more and more attention to the design, construction, and selection of flooring materials. This high requirement is due to the increasing demand for flooring in the industry itself, and on the other hand, it is also a change based on many failed flooring project cases in the past. At the same time, it also shows the importance of flooring as one of the hexahedrons of a building and as a daily human-machine operation platform. The widespread application of steel fiber concrete flooring is mainly to completely replace or partially replace traditional reinforced concrete flooring, which has a greater advantage than traditional steel bars in meeting the needs of industrial plants. Because steel fiber concrete flooring has better crack resistance.
[0003] In actual use of the floor, it was found that the steel fiber concrete floor constructed in the early stage, under the harsh use environment (frequent rolling of vehicles carrying heavy objects, changes in the hot and cold temperature or dry and wet environment of the workshop, and the influence of the working vibration of many equipment), caused the four corners of the steel column base to begin to have cracks of varying degrees. In the case that the floor has been in use for less than two years, it is obvious that it has not met the design and use requirements. Therefore, in order to effectively avoid such floor quality problems and learn from experience, the present invention is designed. Summary of the invention
[0004] The present invention aims at the problems existing in the prior art and proposes an optimized construction method for the steel fiber concrete floor of an industrial plant. By optimizing the specifications of the steel fiber raw materials and adjusting the steel fiber content and the control of the concrete ratio, the large-area steel fiber concrete floor construction is realized and the internal stress of the steel fiber concrete floor is released, the steel fiber concrete floor is prevented from cracking, sanding and possible uneven settlement, and the construction quality is improved. It also plays a significant role in saving construction costs, promoting environmental protection and resource recycling.
[0005] The technical solution adopted by the present invention is: an optimized construction method for steel fiber concrete floor of an industrial plant, which adopts steel fiber concrete for construction, including: Cement, ordinary Portland cement, strength grade 42.5, 475±25 parts; Coarse aggregate, 5-25mm continuously graded crushed stone, alkali-free, 1245±100 parts; Fine aggregate is medium sand, with a solidity index of ≤8%, chloride ion content of ≤0.6%, no alkali activity, 510±50 parts; Admixtures: In winter, the admixtures are 22 parts of early strength agent and 18 parts of air entraining agent. In other seasons, no early strength agent is added. When used in anti-corrosion areas, 18 parts of waterproofing agent and 15 parts of rust inhibitor are added. Steel fiber, steel fiber length 60mm; steel fiber diameter 0.60mm, mixing amount is 15kg / m³; Water, 180 ± 10 parts; The above materials are mixed and stirred to prepare steel fiber concrete, and the slump is controlled at 180-200mm.
[0006] On the basis of the above scheme, as a preferred embodiment, the material properties of the steel fiber are: nominal tensile strength ≥ 1250 MPa, Young's modulus: 200000 N / mm², and ultimate strain: 0.8%.
[0007] Based on the above solution, as a preferred embodiment, before pouring concrete, a plastic film is laid and fixed on the surface of the wall and the column, with a height of not less than 1 meter.
[0008] Based on the above scheme, as a preferred option, after the concrete is in place, the concrete is manually leveled according to the floor elevation reference point, starting with the corners and then the middle.
[0009] Based on the above solution, as a preferred embodiment, a vibrating rod is used to vibrate the concrete while paving, and the vibrating is more frequent at the corners.
[0010] On the basis of the above scheme, as a preferred option, a laser leveler is used to check the leveling immediately after the concrete is vibrated, and then a manual scraper is used for secondary leveling to scrape off the floating slurry and exuded water on the concrete surface. Laser leveling and manual leveling with a scraper should be carried out in the same sequential direction.
[0011] Based on the above solution, preferably, a spatula is used at the corners.
[0012] On the basis of the above scheme, as a preferred embodiment, after the initial setting of the concrete, there are shallow footprints on the surface of the concrete when stepped on. The wear-resistant material is evenly spread in two batches according to the specified amount of wear-resistant material, and the order is as follows: the first time, about 2 / 3 of the wear-resistant material is evenly spread without adding water; after the wear-resistant material absorbs a certain amount of moisture in the concrete, the surface wear-resistant material is in a wet state, and a grinder is used to grind and extract the slurry; after the wear-resistant material hardens, the second spreading operation is carried out, and 1 / 3 of the remaining amount is spread. After the second layer of wear-resistant material absorbs moisture, it is ground again with a grinder. After hardening, the surface is polished with a grinder, and the polishing of the periphery and corner areas of the column base is performed manually.
[0013] Compared with the prior art, the present invention has the following beneficial effects: During the construction of steel fiber flooring with high load-bearing and dynamic load requirements in steel cord plants, the control of raw material ratios can achieve large-area steel fiber concrete flooring construction and release the internal stress of the steel fiber concrete flooring, prevent cracking, sanding and possible uneven settlement of the steel fiber concrete flooring, and improve the construction quality. It also plays a significant role in saving construction costs, promoting environmental protection and resource recycling.
[0014] The selection and mix ratio of raw materials for steel fiber concrete ensure that the steel fiber does not clump when dissolved while maintaining a reasonable density. The floor is durable and has a bright color.
[0015] Compared with concrete floors with steel mesh as the skeleton material, it saves labor and material input to a great extent, greatly reducing construction costs while ensuring the quality of the floor.
[0016] Compared with traditional reinforced concrete floor construction, this construction method greatly speeds up the construction schedule and creates economic benefits for the project to be put into production as soon as possible. DETAILED DESCRIPTION
[0017] The present invention will be further described below by way of examples, but the scope of the present invention is not limited thereto.
[0018] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0019] 1. Cement: Ordinary Portland cement (code PO) with strength grade 42.5 is used. Various indicators (mainly including setting time, stability, mortar strength, magnesium oxide and chloride ion content, and low-alkali cement also needs to test the alkali content) must meet the relevant requirements of "GB175-2020 General Portland Cement".
[0020] 2. Coarse aggregate: 5-25mm continuous graded crushed stone shall be used, and its various indicators (mainly including particle grading, needle-like content, mud content, mud block content, firmness, crushing index) shall meet the requirements of C30 concrete crushed stone in "JGJ52-2006 Standard for Quality and Inspection Methods of Sand and Stone for Ordinary Concrete". In addition, coarse aggregate needs to be tested for alkali activity, and alkali-active aggregate is not allowed.
[0021] 3. Fine aggregate: Use medium sand from Zone II, and its various indicators (mainly including particle grading, mud content or stone powder content, mud block content, firmness, artificial sand crushing value, harmful substance content, chloride ion content) should meet the requirements of C30 concrete sand in "JGJ52-2006 Standard for Quality and Test Methods of Sand and Stone for Ordinary Concrete". Firmness index ≤8%, chloride ion content ≤0.6%. At the same time, the sand needs to be tested for alkali activity, and alkali-active aggregate is also not allowed.
[0022] 4. Admixture: In winter, the admixture is 22 parts of early strength agent and 18 parts of air entraining agent. No early strength agent is added in other seasons. When used in anti-corrosion areas, 18 parts of waterproofing agent and 15 parts of rust inhibitor are added. Various indicators (mainly including water reduction rate, setting time difference, compressive strength ratio, pH value, chloride ion content, alkali content, and air content) must meet the requirements of the current national standards "GB8076 Concrete Admixtures" and "Technical Regulations for Concrete Admixtures". At the same time, the admixture should have good adaptability with cement.
[0023] 5. Steel fiber: The main performance technical parameters are: 1) Material properties: nominal tensile strength ≥ 1250mpa, Young's modulus: 200000N / mm², ultimate strain: 0.8%; 2) Geometric shape: steel fiber series, hooks at both ends; steel fiber length 60mm; steel fiber diameter 0.60mm; aspect ratio (l / d): 100; 3) The product must comply with the A-level standard of GB / T 39147-2020. See Table 1 for specific parameters.
[0024] Table 1 Steel fiber size and tensile strength tolerance
[0025] Among them, the mixing amount of steel fiber and concrete is 15kg / m³. In order to ensure good dispersion and uniformity of steel fibers, steel fibers are bonded into rows with hydrosol. The steel fiber bonding glue adopts special glue for steel fiber materials to ensure the dissolution time of glue in concrete without agglomeration, and strengthen the cohesion between steel fiber and concrete.
[0026] 6. Mixing water: Various indicators of concrete mixing water (mainly including pH value, insoluble matter content, soluble matter content, sulfate ion content, chloride ion content, cement setting time difference and cement-mortar strength ratio) must meet the requirements of "JGJ63 Concrete Water Standard".
[0027] The concrete mix design shall comply with the relevant provisions of "JGJ55-2011 Ordinary Concrete Mix Design Code" and shall meet the concrete construction performance requirements and strength requirements. At the same time, it shall meet: 1. Water-cement ratio: ≤0.5.
[0028] 2. Glue material dosage: cement dosage ≥ 260kg. It is recommended to use cement dosage ≥ 280kg in winter construction. The amount of mineral admixtures should not exceed 25% of the total amount of glue material. The actual dosage is determined based on the test.
[0029] Concrete construction functional requirements: 1. Slump of mixture: 160±20mm for non-pumped concrete and 180±20mm for pumped concrete. These are the slump values of steel fiber concrete when it is transported to the site.
[0030] 2. Setting time: The initial setting time is controlled within 4-6 hours.
[0031] 3. There should not be a large amount of water seepage in the concrete mixture.
[0032] 4. It takes no more than 60 minutes from the time the concrete is mixed out of the machine to the time it is transported to the on-site mold.
[0033] 5. In summer, the temperature of concrete entering the mold should not be higher than 35℃, and in winter, the temperature of concrete entering the mold should not be lower than 5℃.
[0034] Concrete transportation requirements: Concrete is transported by tank trucks (temperature change is guaranteed to be ≤5℃ / h), and the slump of concrete transported to the site must meet the requirements of the mix ratio application form and the opening appraisal. The slump of concrete is measured at the rear of the newly arrived tank truck (one measurement for each truck), and the deviation from the requirement is ±20㎜. The slump of other (special) concrete is notified to the mixing station by the purchaser in the form of an application form based on actual conditions. The concrete mixing station ensures that the concrete transported to the site does not segregate.
[0035] On-site construction requirements: This article only elaborates on the construction of column foot isolation. Steel or wooden formwork is set around the column foot. The top surface of the steel plate is flush with the concrete surface, so that the steel column is partially square (or circular, diamond, etc.) in the floor concrete, which is beneficial to control the occurrence of cracks at the column foot. This part of the area should be poured 14 days after the large area of the outer floor is poured. A 10-15mm thick extruded board is set at the concrete column foot. The extruded board is flush with the floor surface and at the same height as the armor seam to slow down the shrinkage and expansion of the hydrothermal chemical reaction during the concrete pouring. The extruded board needs to be made of environmentally friendly materials and has high compressive resistance, heat insulation performance, corrosion resistance and long-term anti-aging properties. Fiber mesh cloth or metal mesh can also be laid during construction to provide additional support at the concrete stress concentration point (such as wall turning points, window periphery, etc.) to prevent the steel fiber concrete floor from cracking.
[0036] 1. Elevation requirements: The allowable range of elevation error of the column foot floor base is +0 / -15mm. Before pouring concrete, the uneven foundation surface must be trimmed to within the allowable error range. If there are hard spots on the base under the column foot, measures must be taken to ensure that the concrete floor will not crack under load.
[0037] 2. Anti-pollution measures for column edges: To prevent wall panels and steel columns from causing pollution during concrete pouring, plastic film should be laid and fixed on the wall and column surfaces before pouring concrete, with a height of not less than 1 meter.
[0038] 3. On-site management of concrete quality: Concrete slump is an important factor affecting the flatness of the column footing. Therefore, during construction, it is necessary to conduct a slump test on the concrete unloaded into the pouring area, return the concrete that does not meet the requirements, and assist the mixing station to adjust the concrete mix ratio. Carefully observe the dispersion of steel fibers. Once agglomeration or uneven dispersion is found, the concrete cannot be used.
[0039] 4. Concrete pouring, vibration and leveling: After the concrete is in place, the concrete should be roughly leveled manually according to the floor elevation reference point, starting with the corners and then the middle. Use a vibrating rod to vibrate the concrete while leveling it, and vibrate more frequently at the corners. When vibrating, avoid touching the steel bars, core tubes, embedded parts, etc., and do not vibrate close to the board. Immediately after the concrete is vibrated, use a laser leveler to check the leveling. Then use a manual scraper to perform a second leveling to scrape off the slurry and bleeding on the concrete surface to further improve the flatness. At the corners, use a spatula to trim the edges. Note: Laser leveling and manual leveling with a scraper should be performed in a sequential direction to prevent an increase in the exposure of steel fibers.
[0040] 5. Preparation and inspection of steel fiber concrete test blocks: During the construction of steel fiber concrete, the sampling of the slump of the test blocks is subject to the supervision witness system. The steel fiber concrete test blocks are prepared by random sampling on site, and their preparation and maintenance are in accordance with relevant regulations. The construction unit, the supervisor, and the owner participate together. The curing of steel fiber concrete is divided into natural curing and standard curing. The test blocks are cured naturally under the same conditions on site. No standard curing room is set up on site. The prepared test blocks are sent to the testing center for standard curing. The curing temperature is 20.0±2.0℃ and the humidity is ≥90℃. After 28 days of curing, they are allowed to rest and dry under normal conditions. The sampling method and sampling standard of concrete test blocks must meet the relevant requirements of the place where the construction project is located.
[0041] 6. Polishing and finishing: After the initial setting of concrete, there are shallow footprints on the concrete surface when stepped on. According to the specified amount of wear-resistant materials, evenly spread them in two batches in the following order: evenly spread about 2 / 3 of the wear-resistant materials for the first time without adding water; after the wear-resistant materials absorb a certain amount of water in the concrete (the surface wear-resistant materials are once wet), use a polishing machine to grind and extract the slurry; wait for the wear-resistant materials to harden to a certain stage (about 2 hours) for the second spreading operation, and spread 1 / 3 of the remaining amount. After the second layer of wear-resistant materials absorbs a certain amount of water, grind them again with a polishing machine. After hardening to a certain degree, use a polishing machine to polish the surface, and the polishing of the periphery and corner areas of the column foot should be done manually.
[0042] 7. Maintenance: The steel fiber concrete at the column base should be watered and covered with geotextile, and the maintenance time should not be less than 7 days. To ensure the quality of the floor, heavy objects should not be placed during the maintenance period.
[0043] 8. Acceptance of steel fiber concrete floor is divided into flatness acceptance and steel fiber blending acceptance: Among them, flatness acceptance is carried out according to the steel fiber concrete acceptance standards in Table 2:
[0044] Table 2 Acceptance criteria for steel fiber concrete The inspection methods for steel fiber content are water washing method and core sampling method: the water washing method refers to the use of steel fiber content detection equipment to detect the steel fiber content in concrete. Pour 10 liters of steel fiber concrete into the steel fiber content detection equipment, wash the steel fiber sucked out by the magnet with water, dry it and weigh it. The deviation of steel fiber content in a single sample shall not exceed 20% of the mix ratio, and the deviation of the average value of steel fiber content of more than three samples shall not exceed ±10% of the mix ratio; the core sampling method is suitable for ordinary concrete with a strength not exceeding 80MPa. The specific method is to drill cylindrical concrete core samples directly from the structure or component, and conduct a compression test after processing in accordance with relevant specifications, so as to infer the strength of the concrete structure and calculate the steel fiber content based on the compressive strength of the core sample.
[0045] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. An optimized construction method for steel fiber concrete floor of industrial plant, characterized in that: Construction using steel fiber concrete includes: Cement, ordinary Portland cement, strength grade 42.5, 475±25 parts; Coarse aggregate, 5-25mm continuously graded crushed stone, alkali-free, 1245±100 parts; Fine aggregate is medium sand, with a solidity index of ≤8%, chloride ion content of ≤0.6%, no alkali activity, 510±50 parts; Admixtures: In winter, the admixtures are 22 parts of early strength agent and 18 parts of air entraining agent. In other seasons, no early strength agent is added. When used in anti-corrosion areas, 18 parts of waterproofing agent and 15 parts of rust inhibitor are added. Steel fiber, steel fiber length 60mm; steel fiber diameter 0.60mm, mixing amount is 15kg / m³; Water, 180 ± 10 parts; The above materials are mixed and stirred to prepare steel fiber concrete, and the slump is controlled at 180-200mm.
2. The optimized construction method for the steel fiber concrete floor of an industrial plant as claimed in claim 1, characterized in that: Material properties of steel fiber: nominal tensile strength ≥1250mpa, Young's modulus: 200000N / mm², ultimate strain: 0.8%.
3. The optimized construction method for the steel fiber concrete floor of an industrial plant as claimed in claim 1, characterized in that: Before pouring concrete, use plastic film to lay and fix on the surface of walls and columns, with a height of not less than 1 meter.
4. The optimized construction method for the steel fiber concrete floor of an industrial plant as claimed in claim 3 is characterized in that: After the concrete is in place, according to the floor elevation reference point, laser leveling equipment is used and manual labor is used to level the concrete, starting with the corners and then the middle.
5. The optimized construction method for the steel fiber concrete floor of an industrial plant as claimed in claim 4, characterized in that: Use a vibrating rod to vibrate the concrete while leveling it, and vibrate more frequently at the corners to prevent the steel fibers from clumping and ensure that they are evenly distributed.
6. The optimized construction method for the steel fiber concrete floor of an industrial plant as claimed in claim 5, characterized in that: After the concrete is vibrated, use a laser leveler to check the leveling immediately, and then use a manual scraper to perform a second leveling to scrape off the floating slurry and exudate on the concrete surface. Laser leveling and manual leveling with a scraper should be performed in the same sequential direction.
7. The optimized construction method for the steel fiber concrete floor of an industrial plant as claimed in claim 6, characterized in that: At the corners, use a spatula.
8. The optimized construction method for the steel fiber concrete floor of an industrial plant as claimed in claim 6, characterized in that: After the initial setting of the concrete, there are shallow footprints on the surface of the concrete when stepped on. According to the specified amount of wear-resistant materials, they are evenly spread in two batches in the following order: for the first time, about 2 / 3 of the wear-resistant materials are evenly spread without adding water; after the wear-resistant materials absorb a certain amount of moisture in the concrete, the surface wear-resistant materials are wet, and a grinder is used to grind and extract the slurry; after the wear-resistant materials harden, they are spread for the second time, and 1 / 3 of the remaining amount is spread. After the second layer of wear-resistant materials absorbs moisture, it is ground again with a grinder. After hardening, the surface is polished with a grinder, and the polishing of the periphery and corner areas of the column base is done manually.