System and process suitable for suspension roasting of various minerals
By designing a multi-stage cyclone preheating and cooling mineral suspension roasting system, the problems of low processing capacity, high energy consumption and uneven product quality in the existing vertical kiln and rotary kiln processes are solved, and high efficiency and low energy consumption mineral roasting is achieved. , improving automation level and production capacity.
Patent Information
- Application Number
- CN202411339130.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-26
AI Technical Summary
The existing vertical kiln and rotary kiln roasting processes have problems such as low single-machine processing capacity, high energy consumption, long roasting time, uneven product quality, and easy overfire and underfire. It is difficult to effectively deal with a variety of minerals, and the automation level is low.
A mineral suspension roasting system including a suspended roasting furnace, a multi-stage cyclone preheater and cooler, a baking retention tank, a dust collector and a powder conveyor was designed to achieve waste heat recovery through multi-stage preheating and cooling, and a multi-stage cyclone was used. The preheating and cooler series have adjustable baking residence time, which realizes the dispersed state of materials in the airflow and rapid heat and mass transfer.
It has achieved efficient roasting of various minerals, high product quality, low energy consumption, and the dehydration and recovery rate of baked sand reach 99% and above, reducing the problem of knot ring and sintering, suitable for large-scale production, and low equipment maintenance costs , high degree of automation and large production capacity of single furnace.
Smart Images

Figure CN119022648A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral processing, and in particular relates to a system and process suitable for suspension roasting of various minerals. Background Art
[0002] Suspension roasting is a roasting method that makes solid material particles in a fluid state under the action of a fluid medium. It has liquid-like properties. Volatile substances (carbon dioxide, water) in the mineral are removed during the heating process, and then reduced, oxidized or chlorinated in the roasting retention tank to ensure the roasting time. Since most particles are suspended in the gas phase and are in a good dispersion state, the gas and solid are fully in contact, the heat and mass transfer effects are good during the reaction, and the heat consumption is low. The roasting process of the traditional production process is realized in a vertical kiln or a rotary kiln.
[0003] In contrast, the vertical kiln production process is relatively backward. Vertical furnace roasting is mainly suitable for processing lump ore with a particle size of 15 to 75 mm. This process has problems such as low single-machine processing capacity, high energy consumption, long roasting time, uneven product quality, and is prone to over-burning and under-burning.
[0004] Although rotary kiln roasting is suitable for processing ores with smaller particle sizes, problems such as easy ring formation, unstable production, low operating rate and high energy consumption still exist.
[0005] In summary, suspended roasting technology shows obvious advantages in improving product quality, reducing energy consumption, and improving the level of automation, and is of great significance for improving the utilization rate of ore and promoting industrial production. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the present invention provides a mineral suspension roasting system and a roasting process.
[0007] A system suitable for suspension roasting of various minerals, comprising a suspension roasting furnace 9, a primary cyclone preheater 4, a secondary cyclone preheater 5, a third cyclone preheater 6 and a fourth cyclone preheater 7, a roasting retention tank 11, a primary cyclone cooler 14, a secondary cyclone cooler 15, a third cyclone cooler 16, a fourth cyclone cooler 17, a bucket elevator 1, a rotor scale 2, a first air chute 3, a dust collector 18, a high-temperature induced draft fan 19, and a powder conveyor 22;
[0008] The discharge port of the bucket elevator 1 is connected to the feed port of the rotor scale 2 through a chute, and the discharge port of the rotor scale 2 is connected to the feed port of the first air chute 3; the discharge port of the first air chute 3 is connected to the feed port of the first-stage cyclone preheater 4; the first-stage cyclone preheater 4, the second-stage cyclone preheater 5, the third-stage cyclone preheater 6 and the fourth-stage cyclone preheater 7 are connected in sequence through pipelines; the discharge port of the fourth-stage cyclone preheater 7 is connected to the feed port of the suspension roasting furnace 9 through a pipeline, and the discharge port of the cyclone separator 8 connected to the suspension roasting furnace 9 is connected to the feed port of the roasting retention tank 11 through a pipeline. ; The discharge port of the roasting retention tank 11 is connected to the feed port of the primary cyclone cooler 14; the primary cyclone cooler 14, the secondary cyclone cooler 15, the third stage cyclone cooler 16, and the fourth stage cyclone cooler 17 are connected in sequence; the inlet of the dust collector 18 is connected to the exhaust port of the primary cyclone preheater 4 through a pipeline, and the outlet of the dust collector 18 is connected to the high-temperature induced draft fan 19 and the chimney 20 in sequence, and the induced draft fan has its own damper actuator; the ash discharge port of the dust collector 18 is connected to the powder conveyor 22 through the second air chute 21, and the powder conveyor 22 can return the collected ash to the system through pneumatic conveying.
[0009] Furthermore, a first air lock valve 10 is arranged between the cyclone separator 8 and the roasting retention tank 11; a second air lock valve 13 is arranged between the roasting retention tank 11 and the secondary cyclone cooler 15; and a cyclone separator 8 is arranged between the roasting retention tank 11 and the suspension roasting furnace 9.
[0010] A process applicable to suspension roasting of various minerals, using the above system, comprises the following steps:
[0011] Step 1: The raw material is transported to the feed pipe 23 of the primary cyclone preheater 4 via the bucket elevator 1, the rotor scale 2, and the first air chute 3;
[0012] Step 2: The raw material is brought into the primary cyclone preheater 4 by air flow through the feed pipe and separated from the flue gas. It is first mixed with the flue gas from the third-stage cyclone preheater 6 and brought into the second-stage cyclone preheater 5 and separated from the flue gas. It is then mixed with the flue gas from the fourth-stage cyclone preheater 7 and brought into the third-stage cyclone preheater 6 and separated from the flue gas. Finally, it is mixed with the hot flue gas from the suspension roasting furnace and brought into the fourth-stage cyclone preheater 7. The raw material is preheated and pre-roasted to obtain a pre-roasted material. The pre-roasted material is separated from the flue gas here.
[0013] Step 3: The preheated and pre-roasted materials enter the suspension roasting furnace 9 through the pipeline and are roasted in a heated state;
[0014] Step 4: The roasted material enters the roasting retention tank 11 through the cyclone separator 8, the first air lock valve 10 and the pipeline of the suspension roasting furnace. The material undergoes reduction, oxidation and chlorination processes in the roasting retention tank 11, and the roasting retention time is extended. The roasting retention time can be selected from 1 to 240 minutes according to the properties of the material to obtain roasted sand. The number of roasting retention tanks can be selected from 1 to 4 as needed;
[0015] Step 5: The roasted sand is discharged from the roasting retention tank 11 through the second air lock valve 13 and the pipeline into the cooling system for cooling; the cooling is carried out step by step in the first-stage cyclone cooler 14, the second-stage cyclone cooler 15, the third-stage cyclone cooler 16 and the fourth-stage cyclone cooler 17, and the roasted sand can achieve complete countercurrent heat exchange with the cold air, and the cooling air comes from the atmosphere;
[0016] Step 6: The flue gas treatment system is that the dust-containing flue gas from the primary cyclone preheater 4 enters the dust collector 18 through a pipeline for dust removal. A second air chute 21 is provided at the lower part of the dust collector. The collected dust is returned to the system through compressed air and a powder conveyor to realize closed-circuit dust collection; the flue gas after dust removal and purification is sent to the chimney 20 through a high-temperature induced draft fan 19 for discharge.
[0017] Furthermore, the raw material in step 1 is one or more of ferromanganese ore, siderite, limonite, goethite, hematite, complex multiphase mixed iron ore, iron-containing slag, carbon-containing gold ore, stone coal vanadium ore, red mud, aluminum hydroxide, fly ash, limestone ore, spodumene ore, carbide slag, tailings, slag and magnesium ore, and the average particle size of the raw material is less than 1 mm.
[0018] Furthermore, the calcination temperature in step 3 is 500° C. to 1200° C., and the calcination time is 1 to 3 seconds.
[0019] Furthermore, the number of cyclone preheaters and cyclone coolers is selected according to the material roasting temperature, ranging from 1 to 6; the number of cyclone preheater series can be selected according to the material processing capacity, ranging from 1 to 4.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The present invention can widely process various types of minerals, including ferromanganese ore, siderite, limonite, goethite, hematite, complex multiphase mixed iron ore, iron-containing slag, carbon-containing gold ore, stone coal vanadium ore, red mud, aluminum hydroxide, fly ash, limestone ore, spodumene ore, carbide slag, tailings, slag and magnesium ore, so as to realize the comprehensive utilization of resources.
[0022] 2. In the process method of the present invention, the temperature and airflow are evenly distributed, the material is suspended in the airflow in a good dispersion state, heat and mass transfer can be carried out quickly, the reaction rate is fast, and the product quality is high. The heat exchange time of the material in the suspended state is only 1-3 seconds. The material is dehydrated, reduced or oxidized, and the corresponding roasted sand can achieve a dehydration rate of more than 99%, a recovery rate of more than 85%, and a leaching rate of more than 85%.
[0023] 3. The system described in the present invention adopts multi-stage preheating and cooling, has a complete waste heat recovery system, and has low energy consumption per ton of ore.
[0024] 4. The system of the present invention has few production operation problems such as ring formation and sintering, and the roasting residence time can be adjusted, which is suitable for large-scale production.
[0025] 5. The system equipment described in the present invention has fewer operating parts, low maintenance costs, high automation and high operating rate.
[0026] 6. The production capacity of a single furnace in the system of the present invention is very large, which can reach 3.6 million tons of roasted sand per year. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a structural schematic diagram of a novel mineral suspension roasting system of the present invention;
[0028] Among them: 1. bucket elevator; 2. rotor scale; 3. first air chute; 4. first-stage cyclone preheater; 5. second-stage cyclone preheater; 6. third-stage cyclone preheater; 7. fourth-stage cyclone preheater; 8. cyclone separator; 9. suspension roasting furnace; 10. first air lock valve; 11. roasting retention tank; 12. one-way air lock valve; 13. second air lock valve; 14. first-stage cyclone cooler; 15. second-stage cyclone cooler; 16. third-stage cyclone cooler; 17. fourth-stage cyclone cooler; 18. dust collector; 19. high-temperature induced draft fan; 20. chimney; 21. second air chute; 22. powder conveyor; 23. feed pipe. DETAILED DESCRIPTION
[0029] In order to further explain the technical means and effects adopted by the present invention to achieve the intended purpose of the invention, the specific implementation methods, structural features and effects of the present invention are described in detail below in conjunction with the accompanying drawings and preferred embodiments.
[0030] The cyclone preheater of the present invention adopts a single series of four-stage cyclone preheaters, and may also adopt a double series; the cyclone cooler of this embodiment adopts a single series of four-stage cyclone coolers, and may also adopt multiple series. The roasting retention tank described in this embodiment adopts the upper and lower baffle forms.
[0031] A suspension roasting system suitable for various minerals, such as Figure 1As shown, it includes a suspension roasting furnace 9, a primary cyclone preheater 4, a secondary cyclone preheater 5, a third-stage cyclone preheater 6 and a fourth-stage cyclone preheater 7, a roasting retention tank 11, a primary cyclone cooler 14, a secondary cyclone cooler 15, a third-stage cyclone cooler 16, a fourth-stage cyclone cooler 17, a bucket elevator 1, a rotor scale 2, a first air chute 3, a dust collector 18, a high-temperature induced draft fan 19, and a powder conveyor 22;
[0032] The discharge port of the bucket elevator 1 is connected to the feed port of the rotor scale 2 through a chute, and the discharge port of the rotor scale 2 is connected to the feed port of the first air chute 3; the discharge port of the first air chute 3 is connected to the feed port of the first-stage cyclone preheater 4; the first-stage cyclone preheater 4, the second-stage cyclone preheater 5, the third-stage cyclone preheater 6 and the fourth-stage cyclone preheater 7 are connected in sequence through pipelines; the discharge port of the fourth-stage cyclone preheater 7 is connected to the feed port of the suspension roasting furnace 9 through a pipeline, and the discharge port of the cyclone separator 8 connected to the suspension roasting furnace 9 is connected to the feed port of the roasting retention tank 11 through a pipeline; The discharge port of the roasting retention tank 11 is connected to the feed port of the first-level cyclone cooler 14; the first-level cyclone cooler 14, the second-level cyclone cooler 15, the third-level cyclone cooler 16, and the fourth-level cyclone cooler 17 are connected in sequence; the inlet of the dust collector 18 is connected to the exhaust port of the first-level cyclone preheater 4 through a pipeline, and the outlet of the dust collector 18 is connected to the high-temperature induced draft fan 19 and the chimney 20 in sequence, and the induced draft fan has its own damper actuator; the ash discharge port of the dust collector 18 is connected to the powder conveyor 22 through the second air chute 21, and the powder conveyor 22 can return the collected ash to the ash system through pneumatic conveying.
[0033] Furthermore, a first air lock valve 10 is provided between the cyclone separator 8 and the roasting retention tank 11 .
[0034] A process suitable for suspended roasting of various minerals. The raw materials can be ferromanganese ore, siderite, limonite, goethite, hematite, complex multiphase mixed iron ore, iron-containing slag, carbon-containing gold ore, stone coal vanadium ore, red mud, aluminum hydroxide, fly ash, limestone ore, spodumene ore, carbide slag, tailings, slag and magnesium ore, and the average particle size is required to be less than 1 mm.
[0035] Fuels can be coal gas, natural gas, fuel oil, pulverized coal, green hydrogen, biomass, green electricity, etc.
[0036] Example 1
[0037] The chemical composition of the raw materials used in Example 1 is shown in Table 1:
[0038]
[0039] Table 1
[0040] A process applicable to suspension roasting of various minerals, using the above system, comprises the following steps:
[0041] Step 1: The raw material hematite is transported to the feed pipe 23 of the primary cyclone preheater 4 via the bucket elevator 1, the rotor scale 2, and the first air chute 3;
[0042] Step 2: The raw material is brought into the primary cyclone preheater 4 by air flow through the feed pipe 23 and separated from the flue gas. It is first mixed with the flue gas from the third-stage cyclone preheater 6 and brought into the second-stage cyclone preheater 5 and separated from the flue gas. It is then mixed with the flue gas from the fourth-stage cyclone preheater 7 and brought into the third-stage cyclone preheater 6 and separated from the flue gas. Finally, it is mixed with the hot flue gas from the suspension roaster and brought into the fourth-stage cyclone preheater 7. The raw material is preheated and pre-roasted to obtain a pre-roasted material. The pre-roasted material is separated from the flue gas here.
[0043] The fuel is green hydrogen;
[0044] Step 3: The preheated and pre-calcined materials enter the suspension calcining furnace 9 through the pipeline and are calcined in a heated state at a calcination temperature of 850° C. for a calcination time of 1 second;
[0045] Step 4: The roasted material enters the roasting retention tank 11 through the cyclone separator 8, the air lock valve 10 and the pipeline of the suspension roasting furnace, and the material undergoes a reduction process in the roasting retention tank 11. The roasting retention time is 40 minutes to obtain roasted sand, and the chemical composition of the roasted sand is shown in Table 2; the processing capacity is ≤1 million tons / year, and the roasting retention tank is 1; the processing capacity is greater than 1 million tons / year, and the roasting retention tank is 2;
[0046]
[0047] Table 2
[0048] Through the separation process, roasted sand can obtain the technical indicators of iron ore concentrate TFe grade of 65.68% and recovery rate of 91.21%.
[0049] Step 5: The roasted sand is discharged from the roasting retention tank 11 through the one-way air lock valve 12 and the pipeline into the cooling system for cooling; the cooling is carried out step by step in the first-stage cyclone cooler 14, the second-stage cyclone cooler 15, the third-stage cyclone cooler 16 and the fourth-stage cyclone cooler 17, and the roasted sand can achieve complete countercurrent heat exchange with the cold air, and the cooling air comes from the atmosphere;
[0050] The cyclone cooler has 4 cooling stages and the cyclone preheater has 2 preheating stages; if the processing capacity is ≤2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 1; if the processing capacity is between 2 million and 3.2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 2; if the processing capacity is greater than 3.2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 4;
[0051] Step 6: The flue gas treatment system is that the dusty flue gas from the primary cyclone preheater 4 enters the dust collector 18 through the pipeline for dust removal. The lower part of the dust collector is provided with a second air chute 21, and the collected dust is returned to the system through compressed air and a powder conveyor to achieve closed-circuit dust collection. The dust-purified flue gas is sent to the chimney 20 for discharge through a high-temperature induced draft fan 19.
[0052] Example 2
[0053] The chemical composition of the raw materials used in Example 2 is shown in Table 3:
[0054]
[0055] Table 3
[0056] A process applicable to suspension roasting of various minerals, using the above system, comprises the following steps:
[0057] Step 1: The raw material (ferromanganese ore) is transported to the feed pipe of the primary cyclone preheater 4 via the bucket elevator 1, the rotor scale 2, and the first air chute 3;
[0058] Step 2: The raw material is brought into the primary cyclone preheater 4 by air flow through the feed pipe and separated from the flue gas. It is first mixed with the flue gas from the third-stage cyclone preheater 6 and brought into the second-stage cyclone preheater 5 and separated from the flue gas. It is then mixed with the flue gas from the fourth-stage cyclone preheater 7 and brought into the third-stage cyclone preheater 6 and separated from the flue gas. Finally, it is mixed with the hot flue gas from the suspension roasting furnace and brought into the fourth-stage cyclone preheater 7. The raw material is preheated and pre-roasted to obtain a pre-roasted material. The pre-roasted material is separated from the flue gas here.
[0059] The fuel is gas;
[0060] Step 3: The preheated and pre-roasted materials enter the suspension roasting furnace 9 through the pipeline and are roasted in a heated state, where decomposition, oxidation and other processes occur. The roasting temperature is selected according to the type and properties of the raw materials, ranging from a roasting temperature of 950° C. and a roasting time of 2 seconds;
[0061] Step 4: The roasted material enters the roasting retention tank 11 through the cyclone separator 8, the air lock valve 10 and the pipeline of the suspension roasting furnace, and the material undergoes a reduction reaction in the roasting retention tank 11. The roasting retention time is 60 minutes to obtain roasted sand. The chemical composition of the roasted sand is shown in Table 4. If the processing capacity is ≤1 million tons / year, the roasting retention tank is 1; if the processing capacity is >1 million tons / year, the roasting retention tank is 2;
[0062] sample TFe FeO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO MgO P S Mn <![CDATA[Mn 2+ ]]> Burning 600℃ 46.57 18.31 6.06 2.02 0.28 0.32 0.021 0.014 17.56 15.49 0.65
[0063] Table 4
[0064] Through the separation process, roasted sand can obtain manganese concentrate with a Mn grade of 53.36% and an operating recovery rate of 86.98%, and iron concentrate with a TFe grade of 65.40% and an operating recovery rate of 96.59%.
[0065] Step 5: The roasted sand is discharged from the roasting retention tank 11 through the one-way air lock valve 12 and the pipeline into the cooling system for cooling; the cooling is carried out step by step in the first-stage cyclone cooler 14, the second-stage cyclone cooler 15 and the third-stage cyclone cooler 16, and the roasted sand can achieve complete countercurrent heat exchange with the cold air, and the cooling air comes from the atmosphere;
[0066] The cyclone cooler has three-stage cooling and the cyclone preheater has four-stage preheating. If the processing capacity is ≤2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 1; if the processing capacity is between 2 million and 3.2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 2; if the processing capacity is greater than 3.2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 4.
[0067] Step 6: The flue gas treatment system is that the dusty flue gas from the primary cyclone preheater 4 enters the dust collector 18 through the pipeline for dust removal. The lower part of the dust collector is provided with a second air chute 21, and the collected dust is returned to the system through compressed air and a powder conveyor to achieve closed-circuit dust collection. The dust-purified flue gas is sent to the chimney 20 for discharge through a high-temperature induced draft fan 19.
[0068] Example 3
[0069] A process applicable to suspension roasting of various minerals, using the above system, comprises the following steps:
[0070] Step 1: The raw material (aluminum hydroxide Al(OH)3) is transported to the feed pipe of the primary cyclone preheater 4 via a bucket elevator 1, a rotor scale 2, and a first air chute 3;
[0071] Step 2: The raw material is brought into the primary cyclone preheater 4 by air flow through the feed pipe and separated from the flue gas. It is first mixed with the flue gas from the third-stage cyclone preheater 6 and brought into the second-stage cyclone preheater 5 and separated from the flue gas. It is then mixed with the flue gas from the fourth-stage cyclone preheater 7 and brought into the third-stage cyclone preheater 6 and separated from the flue gas. Finally, it is mixed with the hot flue gas from the suspension roasting furnace and brought into the fourth-stage cyclone preheater 7. The raw material is preheated and pre-roasted to obtain a pre-roasted material. The pre-roasted material is separated from the flue gas here.
[0072] The fuel used is fuel oil;
[0073] Step 3: The preheated and pre-roasted materials enter the suspension roasting furnace 9 through the pipeline and are roasted in a heated state, where decomposition, oxidation and other processes occur. The roasting temperature is selected according to the type and properties of the raw materials, ranging from a roasting temperature of 1200° C. and a roasting time of 2 seconds;
[0074] Step 4: The roasted material enters the roasting retention tank 11 through the cyclone separator 8, the air lock valve 10 and the pipeline of the suspension roaster, in which the material undergoes reduction, oxidation and chlorination processes, and the roasting retention time is extended. The roasting retention time can be selected to be 2 minutes according to the material properties to obtain roasted sand (Al2O3). The processing capacity is ≤1 million tons / year, and the roasting retention tank is 1; the processing capacity is>1 million tons / year, and the roasting retention tank is 2; after roasting, the roasted sand dehydration rate can reach 99.3%.
[0075] Step 5: The roasted sand is discharged from the roasting retention tank 11 through the one-way air lock valve 12 and the pipeline into the cooling system for cooling; the cooling is carried out step by step in the first-stage cyclone cooler 14, the second-stage cyclone cooler 15, the third-stage cyclone cooler 16 and the fourth-stage cyclone cooler 17, and the roasted sand can achieve complete countercurrent heat exchange with the cold air, and the cooling air comes from the atmosphere;
[0076] The cyclone cooler has 4 cooling stages and the cyclone preheater has 2 preheating stages. It can be selected according to the material processing capacity. If the processing capacity is ≤2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 1; if the processing capacity is between 2 million and 3.2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 2; if the processing capacity is greater than 3.2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 4.
[0077] Step 6: The flue gas treatment system is that the dusty flue gas from the primary cyclone preheater 4 enters the dust collector 18 through the pipeline for dust removal. The lower part of the dust collector is provided with a second air chute 21, and the collected dust is returned to the system through compressed air and a powder conveyor to achieve closed-circuit dust collection. The dust-purified flue gas is sent to the chimney 20 for discharge through a high-temperature induced draft fan 19.
[0078] Example 4
[0079] The chemical composition of the raw materials used in Example 4 is shown in Table 5:
[0080] Components <![CDATA[Li2O]]> <![CDATA[SiO2]]> <![CDATA[Al2O3]]> TFe CaO MgO <![CDATA[K2O]]> <![CDATA[Na2O]]> Content (wt%) 4.96 55.51 23.2 1.98 0.999 0.53 1.37 0.906
[0081] Table 5
[0082] A process applicable to suspension roasting of various minerals, using the above system, comprises the following steps:
[0083] Step 1: The raw material (spodumene ore) is transported to the feed pipe of the primary cyclone preheater 4 via a bucket elevator 1, a rotor scale 2, and a first air chute 3;
[0084] Step 2: The raw material is brought into the primary cyclone preheater 4 by air flow through the feed pipe and separated from the flue gas. It is first mixed with the flue gas from the third-stage cyclone preheater 6 and brought into the second-stage cyclone preheater 5 and separated from the flue gas. It is then mixed with the flue gas from the fourth-stage cyclone preheater 7 and brought into the third-stage cyclone preheater 6 and separated from the flue gas. Finally, it is mixed with the hot flue gas from the suspension roasting furnace and brought into the fourth-stage cyclone preheater 7. The raw material is preheated and pre-roasted to obtain a pre-roasted material. The pre-roasted material is separated from the flue gas here.
[0085] The fuel is natural gas;
[0086] Step 3: The preheated and pre-calcined materials enter the suspension calcining furnace 9 through the pipeline and are calcined in a heated state at a calcination temperature of 1050° C. for a calcination time of 1 second;
[0087] Step 4: The roasted material enters the roasting retention tank 11 through the cyclone separator 8, the air lock valve 10 and the pipeline of the suspension roasting furnace. In the roasting retention tank 11, the material undergoes a process such as crystal transformation. The roasting residence time is 90 minutes to obtain roasted sand. The processing capacity is ≤1 million tons / year, and the roasting retention tank is 1; the processing capacity is >1 million tons / year, and the roasting retention tanks are 2; the roasted sand crystal conversion rate can reach 99%, the leaching rate is 93.95%, and the leached slag composition is shown in Table 6.
[0088] Components <![CDATA[Li2O]]> <![CDATA[SiO2]]> <![CDATA[Al2O3]]> TFe CaO MgO <![CDATA[K2O]]> <![CDATA[Na2O]]> Content (wt%) 0.287 57.89 21.49 2.11 0.64 0.602 1.44 0.562
[0089] Table 6
[0090] Step 5: The roasted sand is discharged from the roasting retention tank 11 through the one-way air lock valve 12 and the pipeline into the cooling system for cooling; the cooling is carried out step by step in the first-stage cyclone cooler 14, the second-stage cyclone cooler 15, the third-stage cyclone cooler 16 and the fourth-stage cyclone cooler 17, and the roasted sand can achieve complete countercurrent heat exchange with the cold air, and the cooling air comes from the atmosphere;
[0091] The cyclone cooler has 4 cooling stages and the cyclone preheater has 2 preheating stages; if the processing capacity is ≤2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 1; if the processing capacity is between 2 million and 3.2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 2; if the processing capacity is greater than 3.2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 4;
[0092] Step 6: The flue gas treatment system is that the dusty flue gas from the primary cyclone preheater 4 enters the dust collector 18 through the pipeline for dust removal. The lower part of the dust collector is provided with a second air chute 21, and the collected dust is returned to the system through compressed air and a powder conveyor to achieve closed-circuit dust collection. The dust-purified flue gas is sent to the chimney 20 for discharge through a high-temperature induced draft fan 19.
[0093] Example 5
[0094] The chemical composition of the raw materials used in Example 5 is shown in Table 7:
[0095]
[0096]
[0097] Table 7
[0098] A process applicable to suspension roasting of various minerals, using the above system, comprises the following steps:
[0099] Step 1: The raw material (stone coal vanadium ore) is transported to the feed pipe of the primary cyclone preheater 4 via the bucket elevator 1, the rotor scale 2, and the first air chute 3;
[0100] Step 2: The raw material is brought into the primary cyclone preheater 4 by air flow through the feed pipe and separated from the flue gas. It is first mixed with the flue gas from the third-stage cyclone preheater 6 and brought into the second-stage cyclone preheater 5 and separated from the flue gas. It is then mixed with the flue gas from the fourth-stage cyclone preheater 7 and brought into the third-stage cyclone preheater 6 and separated from the flue gas. Finally, it is mixed with the hot flue gas from the suspension roasting furnace and brought into the fourth-stage cyclone preheater 7. The raw material is preheated and pre-roasted to obtain a pre-roasted material. The pre-roasted material is separated from the flue gas here.
[0101] The fuel is pulverized coal;
[0102] Step 3: The preheated and pre-calcined materials enter the suspension calcining furnace 9 through the pipeline and are calcined in a heated state at a calcination temperature of 950° C. for a calcination time of 3 seconds;
[0103] Step 4: The calcined material enters the calcination retention tank 11 through the cyclone separator 8, the air lock valve 10 and the pipeline of the suspension calciner, and the material undergoes a crystal transformation process in the calcination retention tank 11. The calcination retention is 240 minutes to obtain calcined sand. The chemical composition of the calcined sand is shown in Table 8. The processing capacity is ≤1 million tons / year, and the number of calcination retention tanks is 2; the processing capacity is >1 million tons / year, and the number of calcination retention tanks is 4;
[0104] Element <![CDATA[V2O5]]> C <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO MgO TFe content / % 1.05 0.045 68.46 4.41 1.44 0.57 2.48 Element FeO P S K Na Burning content / % 0.53 0.33 0.41 1.49 0.10 -
[0105] Table 8
[0106] The oxidation rate of roasted sand can reach 99.5%, and the leaching rate can reach 85%.
[0107] Step 5: The roasted sand is discharged from the roasting retention tank 11 through the one-way air lock valve 12 and the pipeline into the cooling system for cooling; the cooling is carried out step by step in the first-stage cyclone cooler 14, the second-stage cyclone cooler 15, the third-stage cyclone cooler 16 and the fourth-stage cyclone cooler 17, and the roasted sand can achieve complete countercurrent heat exchange with the cold air, and the cooling air comes from the atmosphere;
[0108] The cyclone cooler has 6 stages of cooling, and the cyclone preheater has 5 stages of preheating. It can be selected according to the material processing capacity. If the processing capacity is ≤ 2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 1; if the processing capacity is between 2 million and 3.2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 2; if the processing capacity is greater than 3.2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 4.
[0109] Step 6: The flue gas treatment system is that the dusty flue gas from the primary cyclone preheater 4 enters the dust collector 18 through the pipeline for dust removal. The lower part of the dust collector is provided with a second air chute 21, and the collected dust is returned to the system through compressed air and a powder conveyor to achieve closed-circuit dust collection. The dust-purified flue gas is sent to the chimney 20 for discharge through a high-temperature induced draft fan 19.
[0110] Example 6
[0111] The chemical composition of the raw materials used in Example 6 is shown in Table 9:
[0112] Components Au* Ag* <![CDATA[SiO2]]> MgO CaO <![CDATA[Al2O3]]> C content / % 3.5 7.1 68.86 2.72 5.55 2.42 6.76 Components TFe S V K Na Ba P content / % 1.31 1.53 0.23 0.49 <0.05 1.11 0.23 Components Mn Cu Zn Hg As Pb Burning content / % 0.014 0.037 0.045 0.0053 0.020 <0.01 13.75
[0113] Table 9
[0114] Note: “*” means unit of g / t.
[0115] A process applicable to suspension roasting of various minerals, using the above system, comprises the following steps:
[0116] Step 1: The raw material (carbon-containing gold ore) is transported to the feed pipe of the primary cyclone preheater 4 via the bucket elevator 1, the rotor scale 2, and the first air chute 3;
[0117] Step 2: The raw material is brought into the primary cyclone preheater 4 by air flow through the feed pipe and separated from the flue gas. It is first mixed with the flue gas from the third-stage cyclone preheater 6 and brought into the second-stage cyclone preheater 5 and separated from the flue gas. It is then mixed with the flue gas from the fourth-stage cyclone preheater 7 and brought into the third-stage cyclone preheater 6 and separated from the flue gas. Finally, it is mixed with the hot flue gas from the suspension roasting furnace and brought into the fourth-stage cyclone preheater 7. The raw material is preheated and pre-roasted to obtain a pre-roasted material. The pre-roasted material is separated from the flue gas here.
[0118] The fuel is biomass;
[0119] Step 3: The preheated and pre-roasted materials enter the suspension roasting furnace 9 through the pipeline and are roasted in a heated state at a roasting temperature of 500° C. for a roasting time of 3 seconds;
[0120] Step 4: The roasted material enters the roasting retention tank 11 through the cyclone separator 8, the air lock valve 10 and the pipeline of the suspension roasting furnace, and the material undergoes an oxidation process in the roasting retention tank 11. The roasting retention is 50 minutes to obtain roasted sand. If the processing capacity is ≤1 million tons / year, there are 2 roasting retention tanks; if the processing capacity is greater than 1 million tons / year, there are 4 roasting retention tanks; the leaching rate of gold in the roasted sand after roasting can reach more than 90%.
[0121] Step 5: The roasted sand is discharged from the roasting retention tank 11 through the one-way air lock valve 12 and the pipeline into the cooling system for cooling; the cooling is carried out step by step in the first-stage cyclone cooler 14, the second-stage cyclone cooler 15, the third-stage cyclone cooler 16 and the fourth-stage cyclone cooler 17, and the roasted sand can achieve complete countercurrent heat exchange with the cold air, and the cooling air comes from the atmosphere;
[0122] The cyclone cooler has 3 cooling stages and the cyclone preheater has 3 preheating stages. It can be selected according to the material processing capacity. If the processing capacity is ≤2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 1; if the processing capacity is between 2 million and 3.2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 2; if the processing capacity is greater than 3.2 million tons / year, the number of cyclone cooler columns and cyclone preheater series is 4.
[0123] Step 6: The flue gas treatment system is that the dusty flue gas from the primary cyclone preheater 4 enters the dust collector 18 through the pipeline for dust removal. The lower part of the dust collector is provided with a second air chute 21, and the collected dust is returned to the system through compressed air and a powder conveyor to achieve closed-circuit dust collection. The dust-purified flue gas is sent to the chimney 20 for discharge through a high-temperature induced draft fan 19.
Claims
1. A system suitable for suspension roasting of various minerals, characterized in that: The invention comprises a suspension roasting furnace (9), a primary cyclone preheater (4), a secondary cyclone preheater (5), a third-stage cyclone preheater (6) and a fourth-stage cyclone preheater (7), a roasting retention tank (11), a primary cyclone cooler (14), a secondary cyclone cooler (15), a third-stage cyclone cooler (16), a fourth-stage cyclone cooler (17), a bucket elevator (1), a rotor scale (2), a first air chute (3), a dust collector (18), a high-temperature induced draft fan (19), and a powder conveyor (22).
2. A system suitable for suspension roasting of various minerals according to claim 1, characterized in that: The discharge port of the bucket elevator (1) is connected to the feed port of the rotor scale (2) through a chute, and the discharge port of the rotor scale (2) is connected to the feed port of the first air chute (3); the discharge port of the first air chute (3) is connected to the feed port of the first-stage cyclone preheater (4); the first-stage cyclone preheater (4), the second-stage cyclone preheater (5), the third-stage cyclone preheater (6) and the fourth-stage cyclone preheater (7) are connected in sequence through pipelines; the discharge port of the fourth-stage cyclone preheater (7) is connected to the feed port of the suspension roasting furnace (9) through a pipeline, and the discharge port of the cyclone separator (8) connected to the suspension roasting furnace (9) is connected to the feed port of the roasting retention tank (11) through a pipeline. ; The discharge port of the roasting retention tank (11) is connected to the feed port of the first-stage cyclone cooler (14); the first-stage cyclone cooler (14), the second-stage cyclone cooler (15), the third-stage cyclone cooler (16), and the fourth-stage cyclone cooler (17) are connected in sequence; the inlet of the dust collector (18) is connected to the exhaust port of the first-stage cyclone preheater (4) through a pipeline, and the outlet of the dust collector (18) is connected to the high-temperature induced draft fan (19) and the chimney (20) in sequence, and the induced draft fan has a damper actuator; the ash discharge port of the dust collector (18) is connected to the powder conveyor (22) through the second air chute (21), and the powder conveyor (22) can return the collected ash to the system through pneumatic conveying.
3. A system suitable for suspension roasting of various minerals according to claim 1, characterized in that: A first air lock valve (10) is arranged between the cyclone separator (8) and the roasting retention tank (11); a second air lock valve (13) is arranged between the roasting retention tank (11) and the secondary cyclone cooler (15); and a cyclone separator (8) is arranged between the roasting retention tank (11) and the suspension roasting furnace (9).
4. A process applicable to suspension roasting of various minerals, using the system according to any one of claims 1 to 3, characterized in that: The steps include: Step 1: The raw material is transported to the feed pipe (23) of the primary cyclone preheater (4) via a bucket elevator (1), a rotor scale (2), and a first air chute (3); Step 2: The raw material is brought into the first-stage cyclone preheater (4) by air flow through the feed pipe and separated from the flue gas. It is first mixed with the flue gas from the third-stage cyclone preheater (6) and brought into the second-stage cyclone preheater (5) and separated from the flue gas. It is then mixed with the flue gas from the fourth-stage cyclone preheater (7) and brought into the third-stage cyclone preheater (6) and separated from the flue gas. Finally, it is mixed with the hot flue gas from the suspension roasting furnace and brought into the fourth-stage cyclone preheater (7). The raw material is preheated and pre-roasted to obtain a pre-roasted material. The pre-roasted material is separated from the flue gas here. Step 3: the preheated and pre-calcined material enters the suspension calcining furnace (9) through a pipeline and is calcined in a heated state at a calcination temperature of 500° C. to 1200° C. for a calcination time of 1 to 3 seconds; Step 4: the roasted material enters the roasting retention tank (11) through the cyclone separator (8), the first air lock valve (10) and the pipeline of the suspension roasting furnace, and the material undergoes reduction, oxidation and chlorination processes in the roasting retention tank (11), and the roasting retention time is extended. The roasting retention time can be selected from 1 to 240 minutes according to the properties of the material to obtain roasted sand. The number of roasting retention tanks can be selected from 1 to 4 according to the needs; Step 5: The roasted sand is discharged from the roasting retention tank (11) through the second air lock valve (13) and the pipeline into the cooling system for cooling; the cooling is carried out step by step in the first-stage cyclone cooler (14), the second-stage cyclone cooler (15), the third-stage cyclone cooler (16) and the fourth-stage cyclone cooler (17), and the roasted sand can achieve complete countercurrent heat exchange with the cold air, and the cooling air comes from the atmosphere; Step 6: The flue gas treatment system is that the dust-containing flue gas from the primary cyclone preheater (4) enters the dust collector (18) through a pipeline for dust removal. The lower part of the dust collector is provided with a second air chute (21). The collected dust is returned to the system through compressed air and a powder conveyor to achieve closed-circuit dust collection; the flue gas after dust removal and purification is sent to the chimney (20) through a high-temperature induced draft fan (19) for exhaust.
5. A process applicable to suspension roasting of various minerals according to claim 4, characterized in that: The raw material in step 1 is one or more of ferromanganese ore, siderite, limonite, goethite, hematite, complex multiphase mixed iron ore, iron-containing slag, carbon-containing gold ore, stone coal vanadium ore, red mud, aluminum hydroxide, fly ash, limestone ore, spodumene ore, carbide slag, tailings, slag and magnesium ore, and the average particle size of the raw material is less than 1 mm.
6. A process applicable to suspension roasting of various minerals according to claim 4, characterized in that: The calcination temperature in step 3 is 500° C. to 1200° C., and the calcination time is 1 to 3 seconds.
7. A process applicable to suspension roasting of various minerals according to claim 4, characterized in that: The number of stages of the cyclone preheater and cyclone cooler is selected according to the material roasting temperature, ranging from 1 to 6; the number of series of the cyclone preheater can be selected according to the material processing capacity, ranging from 1 to 4.