Method and device for testing curing volume change of thermosetting resin in free state

By using the volume change test method and device in the free state during the curing process of thermosetting resin-based composite materials, the problem of limited contribution of volume change test method to residual stress and curing deformation of composite materials in the prior art is solved, and the problem of the volume change test method in the prior art is realized. Accurate measurement and prediction of volume changes of thermosetting resins improve product quality.

CN119023735APending Publication Date: 2024-11-26AVIC BEIJING AERONAUTICAL MFG TECH RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411247962.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing volume change testing methods for thermosetting resin-based composite materials during curing cannot effectively study the residual stress and curing deformation of composite materials, and the constraints of the test device affect the accuracy of the results.

Method used

A method and device for curing volume change testing of thermosetting resin in free state was designed. Using rigid U-shaped grooves, flexible inner bags, strain sensors and temperature sensors, the sensor is buried in the resin through the introduction tube, and the volume change of the resin is recorded to ensure that The resin is in a free state during curing, avoiding constraints and heat accumulation.

Benefits of technology

This method and device can accurately measure the volume change of the thermosetting resin, especially the volume change pattern after gel point, help predict and control the residual stress and curing deformation of the composite material, and improve product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119023735A_ABST
    Figure CN119023735A_ABST
Patent Text Reader

Abstract

The invention relates to a thermosetting resin curing volume change testing method in a free state, which is realized through a thermosetting resin curing volume change testing device in the free state, and the thermosetting resin curing volume change testing device in the free state comprises a rigid U-shaped groove, a flexible inner bag, a strain sensor, a temperature sensor and an ingress pipe, a plurality of holes are formed in the rigid U-shaped groove; the method for testing the curing volume change of the thermosetting resin in the free state comprises the following steps: putting the thermosetting resin to be tested into the flexible inner bag, and then putting the flexible inner bag into the rigid U-shaped groove; the strain sensor and the temperature sensor are embedded in the middle of the thermosetting resin through the ingress pipe, and then the rigid U-shaped groove is placed in a resin curing device; the resin curing process is completed according to the technological process, and the volume change of the thermosetting resin is recorded through the strain sensor and the temperature sensor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of thermosetting resin-based composite materials, and in particular to a method and device for testing the curing volume change of a thermosetting resin in a free state. Background Art

[0002] Thermosetting resin-based composite materials have been widely used in the fields of aviation and aerospace due to their advantages such as high specific stiffness, specific strength, and fatigue properties. However, the residual stress generated inside the material during the manufacturing process of thermosetting resin-based composite materials will lead to serious consequences such as reduced strength, deformation, dimensional changes, cracking, and delamination, and has become a major concern. Regarding the cause of the formation of residual stress during the manufacturing process, researchers believe that in the manufacturing process of thermosetting resin-based composite materials, it is generally believed that the properties of the fiber remain unchanged throughout the process, while the properties of the matrix resin vary with changes in temperature and degree of cure. The behavior of the thermosetting resin matrix, especially the evolution of its volume during the curing process, is one of the main factors in the development of residual stress and strain.

[0003] There are many existing methods for testing the volume change of thermosetting resins during the entire curing cycle, such as measuring the density of resin samples before and after curing, using embedded fiber grating sensors to measure the internal strain of the resin cured in a cylindrical glass container and then converting it into volume change, using the buoyancy principle to measure the volume change of the tested resin during the curing process, and using the volume transfer method to directly measure the volume change of the resin. In these methods, the resin is mostly cured in a relatively rigid container, and the constraints of the test device on the resin matrix are different from the constraints on the actual part in the mold. In addition, the constraints of the test device have a significant impact on the volume change of the resin. Therefore, the results obtained have limited contribution to the study of residual stress and curing deformation of composite parts. Summary of the invention

[0004] (1) Technical issues to be solved

[0005] The present application provides a method for testing the curing volume change of a thermosetting resin in a free state, which solves the problem that the existing method for testing the volume change law of a thermosetting resin during the entire curing cycle has limited contribution to the study of residual stress and curing deformation of composite material parts.

[0006] (2) Technical solution

[0007] In a first aspect, the present application provides a method for testing the curing volume change of a thermosetting resin in a free state, which is implemented by a device for testing the curing volume change of a thermosetting resin in a free state;

[0008] The device for testing the curing volume change of thermosetting resin in a free state comprises a rigid U-shaped groove, a flexible inner bag, a strain sensor, a temperature sensor and an introduction tube, wherein the rigid U-shaped groove is provided with a plurality of holes;

[0009] The method for testing the curing volume change of the thermosetting resin in a free state comprises:

[0010] Putting the tested thermosetting resin into the flexible inner bag, and then putting the flexible inner bag into the rigid U-shaped groove;

[0011] The strain sensor and the temperature sensor are embedded in the middle of the thermosetting resin through the introduction tube, and the rigid U-shaped groove is placed in a resin curing device;

[0012] The resin curing process is completed according to the process flow, and the volume change of the thermosetting resin is recorded by the strain sensor and the temperature sensor.

[0013] Furthermore, the thermosetting resin is any one of epoxy resin, bismaleimide resin, thermosetting polyimide resin, phenolic resin, benzoxazine resin, cyanate resin, unsaturated polyester resin, and vinyl resin.

[0014] Furthermore, after placing the thermosetting resin to be tested into the flexible inner bag and then placing the flexible inner bag into the rigid U-shaped groove, the method further comprises:

[0015] The rigid U-shaped trough is placed in a vacuum oven and evacuated for a period of time to remove air from the thermosetting resin.

[0016] Further, the step of embedding the strain sensor and the temperature sensor into the middle of the thermosetting resin through the introduction tube comprises:

[0017] The strain sensor and the temperature sensor are buried in the thermosetting resin through the introduction tube, and the upper and lower positions of the introduction tube are adjusted so that the sensors are located in the middle of the resin.

[0018] Furthermore, the resin curing device is any one of an oven, an oil bath device, and a water bath device.

[0019] Further, recording the volume change of the thermosetting resin by the strain sensor and the temperature sensor comprises:

[0020] connecting the strain sensor and the temperature sensor to a recording device to record data of the strain and temperature of the thermosetting resin;

[0021] Combined with the change of the temperature of the thermosetting resin over time, a curve of the change of the volume of the thermosetting resin over time and temperature is drawn.

[0022] In a second aspect, the present application provides a device for testing the curing volume change of a thermosetting resin in a free state, which is used to implement the method for testing the curing volume change of a thermosetting resin in a free state as described above;

[0023] The device for testing the curing volume change of a thermosetting resin in a free state comprises a rigid U-shaped groove, a flexible inner bag, a strain sensor, a temperature sensor and an introduction tube, wherein the rigid U-shaped groove is provided with a plurality of holes.

[0024] Furthermore, the width of the rigid U-shaped groove does not exceed 2mm, the wall thickness is 0.5-1mm, and the wall is provided with square or circular holes with a characteristic size of 5-10mm. The material is any one of heat-treated copper alloy, stainless steel, carbon structural steel, and iron.

[0025] Furthermore, the flexible inner bag is made of any one of nylon film, polyethylene film, tetrafluoro film, silicone rubber film and aluminum foil.

[0026] Furthermore, the cross-sectional dimensions of the strain sensor and the temperature sensor do not exceed 1 mm; the inner diameter of the introduction tube is not less than 1.0 mm, and the length is not less than 50 mm.

[0027] (3) Beneficial effects

[0028] The above technical solution of the present application has the following advantages:

[0029] The first aspect of the present application provides a method for testing the curing volume change of thermosetting resin in a free state. The experimental device uses a rigid shell with holes to support a flexible inner bag to hold the resin. The volume change of the thermosetting resin during the curing process is not constrained and is in a free state. The heat can be dissipated through the holes on the rigid shell, which plays a good role in temperature stabilization. The rigid shell is fixed in position during measurement, and the position of the embedded strain sensor is controlled by an introduction tube. The sensor position can be controlled to be in the center of the sample thickness. In this way, the thickness of the resin sample can be small enough so that the heat when the resin is cured and exothermic can be effectively conducted to the surrounding environment, so that the internal temperature of the sample under test does not rise sharply, the amount of resin under test is small, the volume test error is small, and the gel point judgment is more accurate. By studying the volume change of a typical thermosetting resin system during the curing process in a free state, especially the volume change law after the gel point, the curing shrinkage of the thermosetting resin is understood and controlled, thereby providing experimental support for predicting and controlling the residual stress and curing deformation of composite parts and improving product quality.

[0030] It can be understood that the beneficial effects of the second aspect mentioned above can be found in the relevant description of the first aspect mentioned above, and will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0032] Figure 1 A schematic diagram of a rigid U-shaped groove provided for this application;

[0033] Figure 2 Schematic diagram of a test device for curing volume change of a thermosetting resin in a free state provided in the present application;

[0034] Figure 3 Schematic diagram of the curing volume change test of the thermosetting resin in the free state provided in this application.

[0035] Figure numerals: 1. Rigid U-shaped groove; 2. Liquid level of thermosetting resin to be measured; 3. Flexible inner bag; 4. Introduction tube; 5. Sensor. DETAILED DESCRIPTION

[0036] In the following description, specific details such as specific system structures, technologies, etc. are provided for the purpose of illustration rather than limitation, so as to provide a thorough understanding of the embodiments of the present application. However, it should be clear to those skilled in the art that the present application may also be implemented in other embodiments without these specific details. In other cases, detailed descriptions of well-known systems, devices, circuits, and methods are omitted to prevent unnecessary details from obstructing the description of the present application.

[0037] It should be understood that when used in the present specification and the appended claims, the term "comprising" indicates the presence of described features, wholes, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or combinations thereof.

[0038] In addition, in the description of the present application specification and the appended claims, the terms "first", "second", "third", etc. are only used to distinguish the descriptions and cannot be understood as indicating or implying relative importance.

[0039] References to "one embodiment" or "some embodiments" etc. described in the specification of this application mean that one or more embodiments of the present application include specific features, structures or characteristics described in conjunction with the embodiment. Therefore, the statements "in one embodiment", "in some embodiments", "in some other embodiments", "in some other embodiments", etc. that appear in different places in this specification do not necessarily refer to the same embodiment, but mean "one or more but not all embodiments", unless otherwise specifically emphasized in other ways. The terms "including", "comprising", "having" and their variations all mean "including but not limited to", unless otherwise specifically emphasized in other ways. "Multiple" means "two or more".

[0040] The volume shrinkage of thermosetting resin matrix during curing includes two parts. One part is the volume reduction caused by the change from the distance between Van der Waals force to the distance between covalent bonds during the polymerization reaction of the resin when small molecules are converted into a three-dimensional network structure, which is also called "chemical shrinkage". The other part is the volume reduction caused by thermal expansion and contraction during the cooling process of the resin after curing, which is also called "thermal shrinkage". It should be noted that not all chemical shrinkage during curing contributes to dimensional stability and residual stress, because part of the chemical shrinkage occurs before gelation, when the polymer begins to produce mechanical strength and can form a good interface with other components such as reinforcing fibers or strain sensors. Chemical shrinkage after the gel point is called "effective chemical shrinkage". "Effective chemical shrinkage" should be used to calculate the residual stress and deformation caused by curing, otherwise the residual stress and deformation of the composite material will be significantly overestimated.

[0041] In addition, when modeling and numerically analyzing the residual stress and deformation generated during the manufacturing process of composite materials, the effects caused by changes in the material's own properties and state are generally considered separately from the effects caused by the mold. It is very important to understand the volume change of the thermosetting resin matrix in an unconstrained free state. Therefore, studying the volume change of a typical thermosetting resin system during the curing process in a free state, especially the volume change law after the gel point, will help us understand and control the curing shrinkage of thermosetting resins, thereby predicting and controlling the residual stress and curing deformation of composite parts and improving product quality. Most test methods cannot directly determine the occurrence of the gel point, and other test methods such as DSC are required to be used in conjunction, which increases the complexity of the test.

[0042] In response to the above problems, the present application provides a method and device for testing the curing volume change of a thermosetting resin in a free state, which can effectively measure the gel point of the thermosetting resin during curing and the curing volume change in a free state using a small amount of resin.

[0043] The specific implementation methods of the present application are further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present application but are not intended to limit the scope of the present application.

[0044] The method for testing the curing volume change of a thermosetting resin in a free state provided in this embodiment is implemented by a testing device for the curing volume change of a thermosetting resin in a free state. The testing device for the curing volume change of a thermosetting resin in a free state comprises a rigid U-shaped groove, a flexible inner bag, a strain sensor, a temperature sensor and an introduction tube, wherein the rigid U-shaped groove is provided with a plurality of holes.

[0045] The method for testing the curing volume change of the thermosetting resin in a free state comprises: placing the tested thermosetting resin into the flexible inner bag, and then placing the flexible inner bag into the rigid U-shaped groove; burying the strain sensor and the temperature sensor into the middle of the thermosetting resin through the introduction tube, and then placing the rigid U-shaped groove into a resin curing device; completing the resin curing process according to the process flow, and recording the volume change of the thermosetting resin through the strain sensor and the temperature sensor.

[0046] In some embodiments, the thermosetting resin is any one of epoxy resin, bismaleimide resin, thermosetting polyimide resin, phenolic resin, benzoxazine resin, cyanate resin, unsaturated polyester resin, and vinyl resin.

[0047] In some embodiments, after placing the thermosetting resin to be tested into the flexible inner bag and then placing the flexible inner bag into the rigid U-shaped groove, the method further includes: placing the rigid U-shaped groove into a vacuum oven and applying vacuum for a period of time to remove air from the thermosetting resin.

[0048] In some embodiments, burying the strain sensor and the temperature sensor in the middle of the thermosetting resin through the introduction tube includes: burying the strain sensor and the temperature sensor in the thermosetting resin through the introduction tube, and adjusting the upper and lower positions of the introduction tube so that the sensors are located in the middle of the resin.

[0049] In some embodiments, the resin curing device is any one of an oven, an oil bath device, and a water bath device.

[0050] In some embodiments, recording the volume change of the thermosetting resin by the strain sensor and the temperature sensor includes: connecting the strain sensor and the temperature sensor to a recording device to record the strain and temperature data of the thermosetting resin; and drawing a curve of the volume change of the thermosetting resin with time and temperature in combination with the temperature change of the thermosetting resin with time.

[0051] In the application, an experimental device with a rigid U-shaped shell with large holes supporting a flexible inner bag is used to hold the resin, so that the volume change of the tested resin during the curing process is not constrained and is in a free state. The position of the embedded strain sensor is controlled by an inlet tube to obtain the volume change law of the thermosetting resin at the gel point and after the gel point during the curing process in the free state.

[0052] Thermosetting resin refers to epoxy resin or bismaleimide resin or thermosetting polyimide resin or phenolic resin or benzoxazine resin or cyanate resin or unsaturated polyester resin or vinyl resin.

[0053] The test method for the curing volume change of thermosetting resin in the free state, the experimental process is as follows: the tested thermosetting resin is placed in a flexible inner bag with an upper opening, the amount of the tested resin is 15-30g; a U-shaped groove with a width not exceeding 2mm is processed into a metal block as a rigid shell, the wall thickness is 0.5-1mm, and there are square or round holes with a characteristic size of 5-10mm on the wall, such as Figure 1 As shown; then put the flexible inner bag containing the tested resin into the U-shaped groove, so that the thickness of the tested resin does not exceed 2mm; after completing the assembly of the above experimental device, put the experimental device into a vacuum oven and evacuate for 30 minutes to remove the air in the tested resin; put the experimental device after air removal in an oven or an oil bath device or a water bath device, fix the rigid shell on the crossbar, and position the introduction tube at the thickness center of the rigid shell groove, as shown in FIG. Figure 2 shown.

[0054] Adjust the up and down position of the inlet tube so that the sensor is located in the middle of the resin, and fix the up and down position of the inlet tube. Figure 2 As shown in the figure, the strain sensor and the temperature sensor are embedded in the thermosetting resin to be tested through a fixed introduction tube, and the sensor is located in the middle of the resin, as shown in the figure. Figure 3 As shown; the assembled device is placed in an oven or an oil bath, and the resin curing process is completed according to the required process flow. The sensor is connected to a recording device to simultaneously record the strain and temperature data of the tested resin over time at a certain frequency; the measured strain ε is the linear volume change ΔL / L0 of the tested resin. Combined with the change of the temperature data of the tested resin over time, a curve of the linear volume change ΔL / L0 of the tested resin over time and temperature is drawn.

[0055] The present application provides a method for testing the curing volume change of thermosetting resin in a free state. The experimental device of a flexible inner bag supported by a rigid shell with large holes is used to hold the resin. The volume change of the thermosetting resin during the curing process is not constrained and is in a free state. The heat can be dissipated through the large holes on the rigid shell, which plays a good role in temperature stabilization. The rigid shell is fixed in position during measurement, and the position of the embedded strain sensor is controlled by an introduction tube. The sensor position can be controlled to be in the center of the sample thickness. In this way, the thickness of the resin sample can be small enough so that the heat when the resin is cured and exothermic can be effectively conducted to the surrounding environment, so that the internal temperature of the sample under test does not rise sharply, the amount of resin under test is small, the volume test error is small, and the gel point judgment is more accurate. By studying the volume change of a typical thermosetting resin system during the curing process in a free state, especially the volume change law after the gel point, the curing shrinkage of the thermosetting resin is understood and controlled, thereby providing experimental support for predicting and controlling the residual stress and curing deformation of composite parts and improving product quality.

[0056] This embodiment also provides a device for testing the change in cured volume of a thermosetting resin in a free state, which is used to implement the method for testing the change in cured volume of a thermosetting resin in a free state as described above.

[0057] The device for testing the curing volume change of a thermosetting resin in a free state comprises a rigid U-shaped groove, a flexible inner bag, a strain sensor, a temperature sensor and an introduction tube, wherein the rigid U-shaped groove is provided with a plurality of holes.

[0058] In some embodiments, the width of the rigid U-shaped groove does not exceed 2 mm, the wall thickness is 0.5-1 mm, and the wall is provided with square or circular holes with a characteristic size of 5-10 mm. The material is any one of heat-treated copper alloy, stainless steel, carbon structural steel, and iron.

[0059] In some embodiments, the flexible inner bag is made of any one of nylon film, polyethylene film, tetrafluoro film, silicone rubber film, and aluminum foil.

[0060] In some embodiments, the cross-sectional dimensions of the strain sensor and the temperature sensor do not exceed 1 mm; the inner diameter of the introduction tube is not less than 1.0 mm, and the length is not less than 50 mm.

[0061] In the application, the device used to hold the resin is a flexible inner bag supported by a rigid thin shell with holes. The flexible inner bag is made of nylon film, polyethylene film, tetrafluoro film, silicone rubber film or aluminum foil, with an opening at the top, which can hold liquid or slurry fluid and withstand the temperature of resin molding without breaking; the metal block is processed into a U-shaped groove as a rigid outer shell, with a wall thickness of 0.5-1mm and square or round holes with a characteristic size of 5-10mm on the wall. The material is a heat-treated copper alloy, stainless steel, carbon structural steel or iron, which is rigid enough to support the shape of the flexible inner bag and withstand the temperature of resin molding without deformation. The width of the processed U-shaped groove does not exceed 2mm, which is 1mm wider than the maximum characteristic size of the sensor, so that there is a resin layer of about 0.5mm thick on both sides of the sensor to reflect the temperature inside the resin.

[0062] The cross-sectional size of the selected strain sensor and temperature sensor does not exceed 1mm. The strain sensor has a good interface with the resin after the resin is gelled. It does not separate during the curing process after the gel point, and can record the strain and temperature generated by the volume change of the resin at a certain frequency. The inner diameter of the introduction tube is not less than 1.0mm, which can accommodate the strain sensor and temperature sensor to pass through it, and the length is not less than 50mm so that the sensor line remains vertical after passing through it. The volume change law of the thermosetting resin is obtained through the strain measured by the strain sensor and the resin measured by the temperature sensor.

[0063] The following is an explanation through specific embodiments.

[0064] Example 1

[0065] 15g of medium-temperature curing epoxy resin is added to a flexible bag made of polyethylene film with an opening at the top; the flexible bag is placed in a U-shaped groove of a rigid shell made of 0.5mm thick carbon structural steel with 5mm holes, the width of the U-shaped groove is 2mm, and the thickness of the resin in the flexible bag is 2mm; after the experimental device is assembled, the experimental device is placed in a vacuum oven and evacuated for 30 minutes to remove the air in the resin to be tested; after vacuum degassing, the rigid shell is fixed on the cross bar, the introduction tube is placed in the resin and its upper and lower positions are fixed, and the position of the introduction tube is at the center of the thickness of the rigid shell groove; the strain sensor and the temperature sensor are buried in the thermosetting resin to be tested through the introduction tube fixed on the cross bar; the experimental device is placed in an oven, the temperature is increased to 80℃ at a heating rate of 2℃ / min and kept warm for 2h, and the temperature is naturally cooled to room temperature after curing is completed. During the entire process, a fiber Bragg grating sensor with a diameter of 125 μm was used as the strain and a stainless steel-packaged fiber Bragg grating temperature sensor with a diameter of 0.9 mm was connected to a fiber Bragg grating demodulator to record the wavelength peak of the fiber Bragg grating sensor. At the same time, the wavelength peak of the fiber Bragg grating sensor was processed to obtain the curve of the linear volume shrinkage of the resin with time and temperature during the curing process.

[0066] Example 2

[0067] Add 25g of high-temperature curing epoxy resin into a flexible bag made of silicone rubber film with an opening at the top; put the flexible bag into the U-shaped groove of a rigid shell made of a 1mm thick stainless steel sheet with a 10mm hole, the width of the U-shaped groove is 2mm, and the thickness of the resin in the flexible bag is 2mm; after the assembly of the experimental device, put the experimental device into a vacuum oven, and evacuate for 30 minutes to remove the air in the resin to be tested; after vacuum degassing, fix the rigid shell on the cross bar, put the introduction tube into the resin and fix its upper and lower positions, and the position of the introduction tube is at the center of the thickness of the rigid shell groove; bury the strain sensor and the temperature sensor into the thermosetting resin to be tested through the introduction tube fixed on the cross bar; place the experimental device in an oil bath, heat it to 130℃ at a heating rate of 1.5℃ / min, keep it warm for 1h, then heat it to 180℃ at a heating rate of 1℃ / min, keep it warm for 3h, and naturally cool it to room temperature after curing. During the entire process, a fiber Bragg grating sensor with a diameter of 125 μm was used as a strain sensor and a resistance temperature sensor with a diameter of 0.8 mm was used to connect a thermometer and a fiber Bragg grating demodulator to record the temperature and the wavelength peak of the fiber Bragg grating sensor. After processing the data, a curve of the linear volume shrinkage of the resin with time and temperature during the curing process was obtained.

[0068] Those skilled in the art can clearly understand that for the convenience and simplicity of description, only the division of the above-mentioned functional units and modules is used as an example for illustration. In actual applications, the above-mentioned functions can be assigned to different functional units and modules as needed, that is, the internal structure of the device can be divided into different functional units or modules to complete all or part of the functions described above. The functional units and modules in the embodiments can be integrated into one processing unit, or each unit can exist physically separately, or two or more units can be integrated into one unit. In addition, the specific names of the functional units and modules are only for the convenience of distinguishing each other, and are not used to limit the scope of protection of this application.

[0069] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A method for testing the curing volume change of a thermosetting resin in a free state, characterized in that: It is realized by using a test device for curing volume change of thermosetting resin in a free state; The device for testing the curing volume change of thermosetting resin in a free state comprises a rigid U-shaped groove, a flexible inner bag, a strain sensor, a temperature sensor and an introduction tube, wherein the rigid U-shaped groove is provided with a plurality of holes; The method for testing the curing volume change of the thermosetting resin in a free state comprises: Putting the tested thermosetting resin into the flexible inner bag, and then putting the flexible inner bag into the rigid U-shaped groove; The strain sensor and the temperature sensor are embedded in the middle of the thermosetting resin through the introduction tube, and the rigid U-shaped groove is placed in a resin curing device; The resin curing process is completed according to the process flow, and the volume change of the thermosetting resin is recorded by the strain sensor and the temperature sensor.

2. The method for testing the curing volume change of a thermosetting resin in a free state according to claim 1, characterized in that: The thermosetting resin is any one of epoxy resin, bismaleimide resin, thermosetting polyimide resin, phenolic resin, benzoxazine resin, cyanate resin, unsaturated polyester resin and vinyl resin.

3. The method for testing the curing volume change of a thermosetting resin in a free state according to claim 1, characterized in that: After the thermosetting resin to be tested is placed in the flexible inner bag and the flexible inner bag is placed in the rigid U-shaped groove, the method further comprises: The rigid U-shaped trough is placed in a vacuum oven and evacuated for a period of time to remove air from the thermosetting resin.

4. The method for testing the curing volume change of a thermosetting resin in a free state according to claim 1, characterized in that: The step of embedding the strain sensor and the temperature sensor into the middle of the thermosetting resin through the introduction tube comprises: The strain sensor and the temperature sensor are buried in the thermosetting resin through the introduction tube, and the upper and lower positions of the introduction tube are adjusted so that the sensors are located in the middle of the resin.

5. The method for testing the curing volume change of a thermosetting resin in a free state according to claim 1, characterized in that: The resin curing device is any one of an oven, an oil bath device, and a water bath device.

6. The method for testing the curing volume change of a thermosetting resin in a free state according to claim 1, characterized in that: The recording of the volume change of the thermosetting resin by the strain sensor and the temperature sensor comprises: connecting the strain sensor and the temperature sensor to a recording device to record data of the strain and temperature of the thermosetting resin; Combined with the change of the temperature of the thermosetting resin over time, a curve of the change of the volume of the thermosetting resin over time and temperature is drawn.

7. A device for testing the curing volume change of a thermosetting resin in a free state, characterized in that: Used to implement the test method for curing volume change of thermosetting resin in free state according to any one of claims 1 to 6; The device for testing the curing volume change of a thermosetting resin in a free state comprises a rigid U-shaped groove, a flexible inner bag, a strain sensor, a temperature sensor and an introduction tube, wherein the rigid U-shaped groove is provided with a plurality of holes.

8. The device for testing the curing volume change of thermosetting resin in a free state according to claim 7, characterized in that: The width of the rigid U-shaped groove does not exceed 2mm, the wall thickness is 0.5-1mm, and the wall is provided with square or round holes with a characteristic size of 5-10mm. The material is any one of heat-treated copper alloy, stainless steel, carbon structural steel, and iron.

9. The device for testing the curing volume change of thermosetting resin in a free state according to claim 7, characterized in that: The flexible inner bag is made of any one of nylon film, polyethylene film, tetrafluoro film, silicone rubber film and aluminum foil.

10. The device for testing the curing volume change of thermosetting resin in a free state according to claim 7, characterized in that: The cross-sectional dimensions of the strain sensor and the temperature sensor do not exceed 1 mm; the inner diameter of the introduction tube is not less than 1.0 mm, and the length is not less than 50 mm.