Low-temperature sintered conductive silver paste and preparation method and application thereof

By chemically bonding ligands on the surface of silver nanoparticles and using polyolamine crosslinking products as binders, the problem of insufficient conductivity and adhesion of low-temperature conductive silver paste is solved, and high conductivity and good adhesion are achieved, suitable for High precision 3D printing.

CN119028629APending Publication Date: 2024-11-26ENOVATE3D (HANGZHOU) TECH DEV CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310586184.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing low-temperature conductive silver paste has defects in conductivity and adhesion, especially in 3D printing applications, which are difficult to have good conductivity and adhesion, and the often need to add resin binders to lead to poor uniformity and dispersion problems.

Method used

The surface chemical bonding ligand of silver nanoparticles is used, and the ligand-polyolamine cross-linking product is formed as a binder through chemical bonding of polyolamine and ligand, so as to avoid the addition of resin binder and improve conductivity and bondability. , while controlling particle size and dispersion.

Benefits of technology

It achieves the conductivity ≥6.3kS/mm after low temperature sintering at 150-200℃ and ensures adhesion ≥4B, which improves the uniformity and storage stability of the slurry, and is suitable for high-precision 3D printing below 10μm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028629A_ABST
    Figure CN119028629A_ABST
Patent Text Reader

Abstract

The invention relates to the field of conductive paste, in particular to low-temperature sintered conductive silver paste and a preparation method and application thereof, and the low-temperature sintered conductive silver paste comprises silver nanoparticles; ligands are chemically bonded on the surfaces of the silver nanoparticles; the catalyst also comprises a ligand-polyol amine cross-linked product formed by chemical bonding of a ligand and polyol amine. According to the invention, a cross-linked product of polyol amine and a ligand is used as a binder, and the cross-linked product and the ligand are homologous, so that certain cohesiveness can be provided for the slurry, and the problem of dispersity caused by intermiscibility difference cannot be generated; therefore, the conductivity of the silver paste after low-temperature sintering at 150-200 DEG C is not less than 6.3 kS / mm, and the adhesive force of the silver paste to a substrate is not less than 4B. Therefore, the conductive silver paste provided by the invention can be applied to a 3D printing scene with a three-dimensional structure below 10 [mu] m.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of conductive paste, and in particular to a low-temperature sintered conductive silver paste and a preparation method and application thereof. Background Art

[0002] With the rapid development of the electronics industry, the demand for membrane switches, LED displays, and wireless radio frequency identification systems has increased rapidly. Conductive silver paste has attracted extensive attention as a functional material for the preparation of such electronic components due to its excellent conductivity and oxidation resistance. Among them, low-temperature conductive silver paste is widely used in membrane switches, capacitor electrodes, touch screens, etc. due to its excellent conductivity, thermal conductivity, and practicality.

[0003] As metal 3D printing technology matures, compared with traditional processes, it has shown incomparable advantages in shortening the research and development and implementation cycle of new products, efficiently forming more complex structures, achieving integrated and lightweight design, and achieving excellent mechanical properties.

[0004] For example, CN113223748A discloses a low-temperature sintering conductive silver paste, its preparation method and application, wherein the main components of the paste are conductive functional phase metal powder: 70%-80%, silver salt: 1.78%-3.61%, complexing agent: 1.81%-4.77%, organic solvent: 6.62%-16.41%, and resin binder: 5%-15%, wherein the conductive functional phase metal powder is at least one of micron-grade silver powder, nano-grade silver powder or silver-coated copper powder, and the system introduces a silver ion source complex, which can undergo thermal decomposition at 180°C, greatly reducing the sintering temperature of the conductive silver paste; the complex thermally decomposes during the sintering process of the paste to generate silver particles in situ, filling the gaps between the silver powders and playing a "bridge" role, so that the paste and the substrate are tightly connected, a conductive path is formed between the particles, and the resistance value is reduced. However, this system requires the introduction of a resin binder to provide adhesion to the silver paste after sintering. Since the resin is added externally, there will be solubility and dispersibility issues between the resin and the silver powder, resulting in poor uniformity of the paste. Moreover, in order to improve the conductivity of the silver paste, the silver source used in this system is mainly micron-grade silver powder with a large particle size, which limits its application in fields such as 3D printing of precision circuits.

[0005] For example, CN109692971A discloses a nano silver powder and its preparation and application in low temperature curing conductive silver paste. The method for preparing nano silver powder provided uses epoxy resin as a dispersant, one or more of hydrazine hydrate, ascorbic acid and glucose as a reducing agent, and silver ammonia solution as a silver source, and prepares a highly dispersible nano silver powder with a particle size of 50nm-700nm through a reduction reaction. The invention uses epoxy resin as a dispersant, and applies the prepared nano silver powder to a low temperature curing conductive silver paste of the same resin system, which can increase the compatibility of the silver powder and the resin in the low temperature curing conductive silver paste, thereby improving the conductivity of the paste. However, the patent uses epoxy resin as a dispersant and a subsequent binder. Since epoxy resin is a type of insulating resin, it will seriously affect the conductivity of the low temperature silver paste. In addition, the invention uses a process of multiple water washing and alcohol washing in the washing process, which will cause the agglomeration problem caused by the lack of ligands on the particle surface in the paste. At the same time, there will be problems such as insufficient surface density after sintering and low surface sintering activity, which directly affects its product performance.

[0006] For example, CN106623971A discloses a nano silver particle for conductive ink and a preparation method thereof, wherein the preparation method of the silver nano particles is to first add a silver source, a coating agent and an organic amine solution to a solution, add a reducing agent to carry out a reduction reaction, wash and dry to obtain the nano silver particles. This method can obtain nano silver particles of 50-70nm. SEM shows that the obtained silver nano particles have a uniform particle size, good dispersibility, and are not easy to agglomerate. The nano silver particles obtained by the patent scheme can be applied to low-temperature silver paste, but due to the lack of corresponding binders to provide adhesion, its application is limited. Moreover, the subsequent slurry washing process of the patent is to centrifuge and wash 3 times with deionized water and ethanol respectively, which will lead to the problem of agglomeration and uneven dispersion due to the lack of ligands on the surface of the silver particles in the subsequent slurry configuration process.

[0007] The application of low-temperature conductive silver paste in 3D printing often requires excellent properties in terms of conductivity and adhesion, and also has high requirements for particle size control. Currently, the existing low-temperature conductive silver paste often needs to be improved in these aspects. How to develop a low-temperature conductive silver paste with good conductivity and adhesion that can be used in 3D printing is a technical problem that needs to be solved urgently in this technical field. Summary of the invention

[0008] In order to overcome the defects of low-temperature conductive silver paste in the prior art in terms of conductivity and adhesion, the present invention provides a low-temperature sintered conductive silver paste and a preparation method and application thereof to overcome the above-mentioned shortcomings.

[0009] To achieve the above-mentioned purpose, the present invention is implemented by the following technical solutions: In a first aspect, the present invention first provides a low-temperature sintering conductive silver paste. It includes silver nanoparticles; The silver nanoparticles have ligands chemically bonded to their surfaces; Also included are ligand-polyol amine cross-linked products formed by chemical bonding of the ligand and the polyol amine.

[0010] As described in the background art, in addition to the conventional conductive phase (such as the nano silver particles in the present application), the conductive paste in the prior art usually needs to add a certain amount of resin binder to the paste in order to ensure the adhesion of the conductive phase to the substrate after sintering. However, due to the poor compatibility between the resin binder and the conductive phase, the dispersibility of the conductive phase in the resin binder is poor, resulting in the problem of easy agglomeration of the nano-scale conductive phase during the dispersion process. At the same time, the resin binder in the prior art is usually an epoxy resin with poor conductivity, and the corresponding silver paste has poor conductivity. Therefore, the current conductive paste has the following technical problems, namely: the paste with good adhesion after low-temperature sintering at 150-200°C has relatively poor conductivity, with a conductivity of <6.3kS / mm; and the paste with good conductivity after low-temperature sintering at 150-200°C, that is, the low-temperature silver paste with a conductivity of ≥6.3kS / mm, has no suitable binder to provide corresponding adhesion while ensuring its conductivity. Therefore, the key point of the present invention is to improve the adhesion and conductivity of the conductive silver paste while ensuring the uniformity of the paste.

[0011] The low-temperature sintering conductive silver paste of the present invention mainly comprises two parts, namely, silver nanoparticles and a ligand-polyol amine cross-linked product.

[0012] Regarding silver nanoparticles, the silver nanoparticles in the prior art usually do not have corresponding ligands on their surfaces or the ligands are lost during the preparation and purification process, which makes the exposed silver atoms or ions on the surface of the silver particles more susceptible to electrostatic adsorption, thereby easily causing the problem of agglomeration. The silver nanoparticles in the present invention still have ligands chemically bonded to their surfaces when they are in the slurry, and these ligands can prevent electrostatic adsorption between adjacent silver nanoparticles, thereby preventing the occurrence of agglomeration.

[0013] Regarding the ligand-polyol amine cross-linked product, the ligand in the ligand-polyol amine cross-linked product of the present invention has the following two situations: (1) This type of ligand refers to the free ligand in the system after the reaction of the silver nanoparticles is completed. In this case, it is only necessary to directly add polyol amine to the synthesis system after the synthesis of the silver nanoparticles. The polyol amine directly reacts with the active functional groups in the ligands that are still free in the system to obtain the ligand-polyol amine cross-linked product. That is, the final slurry contains both silver nanoparticle-ligand and ligand-polyol amine cross-linked product.

[0014] (2) This type of ligand refers to an additional ligand that is the same as the ligand on the surface of the silver nanoparticles. The ligand is cross-linked with polyol amine alone to obtain the corresponding ligand-polyol amine cross-linked product. The ligand-polyol amine cross-linked product is then purified and mixed with the silver nanoparticles in a suitable ratio, that is, the final slurry contains both silver nanoparticle-ligand and ligand-polyol amine cross-linked product. The silver nanoparticle-ligand part has been discussed in the above discussion, and it has been shown that the aggregation of silver nanoparticles will be significantly reduced after the ligand is chemically bonded to the surface. At the same time, the present invention also has a ligand-polyolamine cross-linked product. Since the ligand-polyolamine cross-linked product and the silver nanoparticles both contain the same ligand, the compatibility between the silver nanoparticle-ligand and the ligand-polyolamine cross-linked product in the present application can be greatly improved. When the two are mixed, the silver nanoparticles containing the ligand in the present application can be effectively dispersed in the cross-linked product, and there will be no sedimentation and agglomeration. Therefore, after the slurry is prepared, the uniformity and storage stability of each part of the slurry can be effectively improved, thereby improving the density and conductivity of the film surface after the slurry is sintered, so that the slurry will not change after long-term storage. At the same time, the ligand-polyolamine cross-linked product itself also has a certain degree of cross-linking, so its bonding performance is good, so there is no need to add exogenous bonding resin in the conductive slurry configuration process, so that the conductive silver slurry can provide corresponding bonding while ensuring its conductivity after curing and sintering.

[0015] Finally, the ligand-polyolamine cross-linked product of the present invention contains a polyolamine structure, which has a certain reducing property. Therefore, during the storage of the conductive silver paste, it can ensure that the nanosilver particles mixed therewith will not be oxidized, thereby ensuring the stability of the conductive performance of the conductive silver paste after solidification and sintering.

[0016] Preferably, the low-temperature sintering conductive silver paste also includes a diluent.

[0017] Preferably, the silver paste comprises the following components by mass percentage: 65-95% of silver nanoparticles, 2-10% of ligand-polyol amine cross-linked product and 3-25% of diluent.

[0018] In existing conductive pastes, low-boiling-point organic solvents generally account for a high proportion, which can easily lead to linear shrinkage and slurry leveling problems after heating during the sintering process, resulting in cracks and collapse during the sintering process. The low-volatile solvent content in the system of the present invention is low, so during the curing process, the shrinkage rate of the circuit is lower and its conformality is better.

[0019] Preferably, the ligand is an unsaturated organic acid polymer having the general structural formula shown in the following formulas (Ⅰ), (Ⅱ), and (Ⅲ); Formula (I): Formula (II): Formula (III): Wherein: R1, R2, R3 are alkyl or H.

[0020] In the present invention, the unsaturated organic acid polymer containing the above structural formula is selected as the ligand of the silver nanoparticles, which can effectively adhere to the surface of the silver nanoparticles, thereby controlling the particle size of the generated silver nanoparticles during the preparation of the silver nanoparticles and can be used as a protective agent to protect the silver nanoparticles. At the same time, since the structure contains a carboxyl group, it can be cross-linked with a reducing agent alcohol amine substance to obtain the desired cross-linked product as a binder.

[0021] Preferably, the ligand is a combination of any one or more of polyacrylic acid, polymethacrylic acid, polymaleic acid, maleic acid-acrylic acid copolymer and homologues thereof.

[0022] Preferably, the ligand is polyacrylic acid with a molecular weight between 3000 and 200000.

[0023] Preferably, the diluent is a solvent with a carbon number / hydroxyl group ≤4 and a hydroxyl group number ≥2.

[0024] The diluent in the present invention selects a compound with a polyhydroxy structure because the compound with a polyhydroxy structure can form an unstable cross-linked hydrogen bond with the other components in the system. During storage, this part of the hydrogen bond can ensure that each component in the system can remain stable, so that the storage stability of the conductive silver paste is greatly improved. During use, the effect of this part of the hydrogen bond will not be too strong to affect the actual printing. At the same time, the boiling point of these compounds is significantly improved compared to monohydroxy compounds, so there will be no problem of excessive volatilization and system changes during actual use.

[0025] Preferably, the diluent includes any one or more combinations of water, ethylene glycol, glycerol, 1,4-butanediol, isoprene glycol, and trimethylolpropane.

[0026] Preferably, the polyol amine has a general chemical formula of (CH2) a (OH) b NH secondary alcohol amine or chemical formula (CH2) a (OH) b Any one or more combinations of tertiary alcohol amines of N; Among them: 2≤a / b≤6, 2≤b≤6.

[0027] The present invention adopts a ligand-polyol amine cross-linked product as a binder. The principle is that the polyol amine and the above-mentioned ligand can form a cross-linked network structure during the mixing reaction. Therefore, the ligand-polyol amine cross-linked product finally obtained can have a good coating, dispersion and protection effect on silver nanoparticles.

[0028] Preferably, the polyol amine is any one or more combinations of diethanolamine, triethanolamine, diisopropanolamine and triisopropanolamine.

[0029] In a second aspect, the present invention further provides a method for preparing the low temperature sintering conductive silver paste as described above, comprising the following steps: (S.1) mixing a silver salt solution with a ligand solution, and using a monohydric alcohol amine as a reducing agent to react to obtain a liquid phase system including silver nanoparticles with surface chemically bonded ligands and free ligands; (S.2a) adding a polyol amine to the liquid phase system obtained in step (S.1) to allow the free ligand to undergo a cross-linking reaction with the polyol amine to obtain a ligand-polyol amine cross-linked product, and finally purifying the entire system using a purification solvent to obtain the low-temperature sintering conductive silver paste; or, (S.2b) The liquid phase system obtained in step (S.1) is purified by a purification solvent to obtain silver nanoparticles with surface chemically bonded ligands, the ligands are mixed with polyol amines and heated to form ligand-polyol amine cross-linked products, and the silver nanoparticles with surface chemically bonded ligands and the ligand-polyol amine cross-linked products are evenly mixed to obtain the low-temperature sintering conductive silver paste. (S.3) adding a diluent to the low temperature sintering conductive silver paste to adjust the viscosity of the low temperature sintering conductive silver paste.

[0030] In the present invention, in (S.1), monoalcohol amine is used as a reducing agent. On the one hand, the reducing property of monoalcohol amine is significantly higher than that of polyalcohol amine, and the synthesis of nano silver particles can be effectively realized; on the other hand, it is not easy to form a cross-linked product with the ligand, so it can ensure that the nano silver particles are fully coated with the ligand to obtain a silver nano particle-ligand complex with uniform morphology. Afterwards, in order to obtain the low temperature sintering conductive silver paste, its main steps can be divided into two steps including the preparation of silver nano particles and the cross-linking step of the ligand and the polyalcohol amine.

[0031] As described above, there are two ways to introduce the ligand-polyol amine cross-linked product into the slurry of the present invention. Therefore, for these two ways, step (S.2) of the present invention also includes two different preparation methods.

[0032] Wherein (S.2a): for the case where the ligand refers to the free ligand in the system after the reaction of the silver nanoparticles is completed, in this case, it is only necessary to directly add polyol amine to the synthesis system after the synthesis of the silver nanoparticles, and the polyol amine directly reacts with the active functional groups in the ligands that are still free in the system. After this process is completed, a suitable purification solvent is selected to purify the cross-linked product as a whole to obtain the corresponding conductive silver paste, and the purification process can remove excess reducing agents and other impurities. In addition, (S.2b) for the case where this type of ligand refers to the additionally added ligand of the same type as the surface of the silver nanoparticles, in this case, the present invention first selects a suitable purification solvent to purify the synthesized silver nanoparticles, and obtains a nanosilver particle-ligand complex after purification, and removes the free ligand, excess reducing agent and other impurities. At the same time, the ligand is cross-linked with the polyol amine alone to obtain the corresponding ligand-polyol amine cross-linked product, and then the ligand-polyol amine cross-linked product is purified and mixed with the silver nanoparticles in a suitable ratio to obtain the corresponding conductive silver paste.

[0033] There have been precedents in the prior art of using polyol amines as reducing agents to obtain silver nanoparticles, but the silver paste obtained by this method often has poor conductivity after low-temperature sintering. As shown in the literature (BY Ahn, EBD Duoss, MJ Motala, X. Guo, S. Park, Y. Xiong, J. Yoon, RG Nuzzo, JA Rogers, JA Lewis, Science, 2009, 323, 1590-1593, DOI: 10.1126 / science.1168375), a higher conductivity can only be obtained under high temperature conditions above 500°C. The reason is that in the process of reducing silver ions to form silver nanoparticles, polyol amine is easy to produce cross-linking reaction with ligand at the same time, so the obtained product will be a composite of silver nanoparticles-ligand-polyol amine, and its ligand will be cross-linked with silver nanoparticles and polyol amine at the same time. Since the composite of silver nanoparticles-ligand-polyol amine obtained in this way is difficult to decompose at low temperature, the sintering effect of conductive silver paste at low temperature is poor. Under normal conditions, it can only be sintered at a temperature above 300°C to obtain a higher conductivity. In the present invention, low-boiling point alcohol amine is used as a reducing agent, so that there is no silver nanoparticle-ligand-polyol amine composite on the surface of the obtained silver nanoparticles, and only two forms of silver nanoparticles-ligand and ligand-polyol amine exist. Therefore, the conductivity of ≥6.3kS / mm can be obtained by low-temperature sintering at a relatively low temperature such as 150°C.

[0034] Preferably, the monohydric alcohol amine has the general formula OH-X-NH2, wherein X is an alkane chain with 2≤carbon number≤6.

[0035] Preferably, the monoalcoholamine is a combination of one or more of ethanolamine, propanolamine, isopropanolamine and isobutanolamine.

[0036] Preferably, the purification solvent includes a good solvent containing a hydroxyl group or a carbonyl group; and a sub-good solvent containing an ester group.

[0037] The present invention effectively reduces the retention rate of impurities in the conductive silver paste by optimizing the purification method. The purification method in the present invention is to select a purification solvent composed of a good solvent with a strong solubility for the ligand and a sub-good solvent with a weak solubility for the ligand. This purification solvent can effectively remove free ligands during the purification process by adjusting the polarity of the purification solvent, while ensuring that the ligands on the surface of the silver nanoparticles are not removed, ensuring the stability of the slurry during storage and the surface density after sintering, and improving the overall stability of the slurry and the conductive performance after sintering.

[0038] Preferably, the good solvent is any one of methanol, ethanol, acetone or a combination thereof.

[0039] Preferably, the sub-good solvent is any one of ethyl acetate, propyl acetate, butyl acetate or a combination thereof.

[0040] On the third aspect, the present invention also provides the application of the low-temperature sintered conductive silver paste or the low-temperature sintered conductive silver paste prepared by the above method in high-precision direct writing 3D printing of 10 μm and below, precision optics, micro-nano chips, photovoltaics or printed electronics.

[0041] Therefore, the present invention has the following beneficial effects: (1) It can ensure that the conductivity of the silver paste is ≥6.3kS / mm after low-temperature sintering at 150-200℃, and at the same time ensure that the adhesion of the silver paste to the substrate after sintering is ≥4B.

[0042] (2) The silver nanoparticles in the silver paste are synthesized by an aqueous phase synthesis method, and a cross-linked product of a polyol amine and a ligand is selected as a binder. The cross-linked product is homologous to the ligand, which can provide a certain degree of adhesion to the paste without causing dispersion problems due to differences in compatibility.

[0043] (3) The silver paste in this application can be applied to 3D printing scenarios of three-dimensional structures below 10 μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is a SEM photograph of the silver particles in the nano silver paste (A1) prepared in Example 1.

[0045] Figure 2This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A1) prepared in Example 1.

[0046] Figure 3 This is a SEM photograph of the silver particles in the nano silver paste (A2) prepared in Example 2.

[0047] Figure 4 This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A2) prepared in Example 2.

[0048] Figure 5 This is a SEM photograph of the silver particles in the nano silver paste (A3) prepared in Example 3.

[0049] Figure 6 This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A3) prepared in Example 3.

[0050] Figure 7 This is a SEM photograph of the silver particles in the nano silver paste (A4) prepared in Example 4.

[0051] Figure 8 This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A4) prepared in Example 4.

[0052] Fig. 9 This is a SEM photograph of the silver particles in the nano silver paste (A5) prepared in Example 5.

[0053] Fig.10 This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A5) prepared in Example 5.

[0054] Fig.11 This is a SEM photograph of the silver particles in the nano silver paste (A6) prepared in Example 6.

[0055] Fig.12 This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A6) prepared in Example 6.

[0056] Fig.13 This is a SEM photograph of the silver particles in the nano silver paste (A7) prepared in Example 7.

[0057] Fig.14 This is a SEM photograph of the silver film obtained after sintering the nanosilver paste (A7) prepared in Example 7.

[0058] Fig.15 This is a SEM photograph of the silver particles in the nano silver paste (A8) prepared in Example 8.

[0059] Fig.16This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A8) prepared in Example 8.

[0060] Fig.17 This is a SEM photograph of silver particles in the nano silver paste (A9) prepared in Example 9.

[0061] Fig.18 This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A9) prepared in Example 9.

[0062] Fig.19 This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A10) prepared in Example 10.

[0063] Fig. 20 This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A11) prepared in Example 11.

[0064] Fig.21 This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A12) prepared in Example 12.

[0065] Fig. 22 This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A13) prepared in Example 13.

[0066] Fig.23 This is a SEM photograph of the silver film obtained after sintering the nanosilver paste (A14) prepared in Example 14.

[0067] Fig.24 This is a SEM photograph of the silver film obtained after sintering the nano silver paste (A15) prepared in Example 15.

[0068] Fig.25 This is a SEM photograph of the silver particles in the nano silver paste (D1) prepared in Comparative Example 1.

[0069] Fig.26 This is a SEM photograph of the silver film obtained after sintering the nanosilver paste (D1) prepared in Comparative Example 1.

[0070] Fig. 27 This is a SEM photograph of the silver particles in the nanosilver paste (D2) prepared in Comparative Example 2.

[0071] Fig.28 This is a SEM photograph of the silver film obtained after sintering the nanosilver paste (D2) prepared in Comparative Example 2.

[0072] Fig.29 This is a SEM photograph of the silver particles in the nano silver paste (D3) prepared in Comparative Example 3.

[0073] Fig.30 This is a SEM photograph of the silver film obtained after sintering the nanosilver paste (D3) prepared in Comparative Example 3.

[0074] Fig.31 This is a SEM photograph of the silver particles in the nanosilver paste (D4) prepared in Comparative Example 4.

[0075] Fig.32 This is a SEM photograph of the silver film obtained after sintering the nanosilver paste (D4) prepared in Comparative Example 4.

[0076] Fig.33 This is a SEM photograph of the silver film obtained after sintering the nanosilver paste (D5) prepared in Comparative Example 5.

[0077] Fig.34 This is a SEM photograph of the silver film obtained after sintering the nanosilver paste (D6) prepared in Comparative Example 6.

[0078] Fig.35 This is a SEM photograph of the silver film obtained after sintering the nanosilver paste (D7) prepared in Comparative Example 7. DETAILED DESCRIPTION

[0079] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments of the specification. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0080] Example 1 A method for preparing a low-temperature sintered conductive silver paste comprises the following steps: (1) Take 20g AgNO3 (118mmol) and dissolve it in 20g deionized water to prepare a silver nitrate solution. Add 50g deionized water into a conical flask, then add 3g PAA (MW 3000) and 1g PAA (MW 20,000) in sequence, start stirring, and drop the silver nitrate solution into the conical flask. Finally, pour 14.4g (236mmol) ethanolamine into the conical flask at a faster rate and stir at 300r / min for 2h. (2) Heat and stir on a hot plate at 120°C for 2 h, then pour 6.2 g (59 mmol) of diethanolamine into the conical flask and continue heating and stirring for 2 h; (3) Cool to room temperature, add 100 ml of ethyl acetate, then add 300 ml of ethanol in portions, stir for 10 min, the product will precipitate as flocculent, remove the supernatant, transfer the precipitate to a 50 ml centrifuge tube, and centrifuge at 9000 rpm for 20 min; (4) The supernatant was removed, deionized water was added to 15 mL, and the mixture was shaken evenly. 10 mL of ethyl acetate was added, and then 50 mL of ethanol was added and shaken evenly. The mixture was centrifuged at 9000 rpm for 20 min, the supernatant was removed, and the mixture was mixed to obtain a nanosilver paste (A1). The SEM photograph of the silver particles is shown in FIG. Figure 1 The particle size is <400nm. The SEM photo of the silver film obtained after sintering is shown in FIG. Figure 2 shown.

[0081] Example 2 A method for preparing a low-temperature sintered conductive silver paste comprises the following steps: (1) Take 20g AgNO3 (118mmol) and dissolve it in 20g deionized water to prepare a silver nitrate solution. Add 50g deionized water into a conical flask, then add 3g PAA (MW 5000) and 1g PAA (MW 100,000) in sequence, start stirring, and add the silver nitrate solution dropwise into the conical flask. Finally, pour 14.4g (236mmol) ethanolamine into the conical flask at a faster rate and stir at 300r / min for 2h. (2) Heat and stir on a hot plate at 120°C for 2 h, then pour 6.2 g (59 mmol) of diethanolamine into the conical flask and continue heating and stirring for 2 h; (3) Cool to room temperature, add 100 ml of ethyl acetate, then add 300 ml of ethanol in portions, stir for 10 min, the product will precipitate as flocculent, remove the supernatant, transfer the precipitate to a 50 ml centrifuge tube, and centrifuge at 9000 rpm for 20 min; (4) The supernatant was removed, deionized water was added to 15 mL, and the mixture was shaken evenly. 10 mL of ethyl acetate was added, and then 50 mL of ethanol was added and shaken evenly. The mixture was centrifuged at 9000 rpm for 20 min, and the supernatant was removed and mixed to obtain a nanosilver paste (A2). The SEM photograph of the silver particles is shown in FIG. Figure 3 The particle size is <500nm. The SEM photo of the silver film obtained after sintering is shown in Figure 4 shown.

[0082] Example 3 A method for preparing a low-temperature sintered conductive silver paste comprises the following steps: (1) Take 20g AgNO3 (118mmol) and dissolve it in 20g deionized water to prepare a silver nitrate solution. Add 50g deionized water into a conical flask, then add 3g PAA (MW 5000) and 1g PAA (MW 200,000) in sequence, start stirring, and add the silver nitrate solution dropwise into the conical flask. Finally, pour 14.4g (236mmol) ethanolamine into the conical flask at a relatively fast rate and stir at 300r / min for 2h. (2) Heat and stir on a hot plate at 120°C for 2 h, then pour 6.2 g (59 mmol) of diethanolamine into the conical flask and continue heating and stirring for 2 h; (3) Cool to room temperature, add 100 ml of ethyl acetate, then add 300 ml of ethanol in portions, stir for 10 min, the product will precipitate as flocculent, remove the supernatant, transfer the precipitate to a 50 ml centrifuge tube, and centrifuge at 9000 rpm for 20 min; (4) The supernatant was removed, deionized water was added to 15 mL, and the mixture was shaken evenly. 10 mL of ethyl acetate was added, and then 50 mL of ethanol was added and shaken evenly. The mixture was centrifuged at 9000 rpm for 20 min, and the supernatant was removed and mixed to obtain a nanosilver paste (A3). The SEM photograph of the silver particles is shown in FIG. Figure 5 The particle size is <600nm. The SEM photo of the silver film obtained after sintering is shown in Figure 6 shown.

[0083] Example 4 A method for preparing a low-temperature sintered conductive silver paste comprises the following steps: (1) Take 20 g of AgNO3 (118 mmol) and dissolve it in 20 g of deionized water to prepare a silver nitrate solution. Add 50 g of deionized water into a conical flask, then add 4 g of maleic acid-acrylic acid copolymer (MW 3000) in sequence, start stirring, and drop the silver nitrate solution into the conical flask. Finally, pour 14.4 g (236 mmol) of ethanolamine into the conical flask at a faster rate and stir at 300 r / min for 2 h. (2) Heat and stir on a hot plate at 120°C for 2 h, then pour 6.2 g (59 mmol) of diethanolamine into the conical flask and continue heating and stirring for 2 h; (3) Cool to room temperature, add 100 ml of ethyl acetate, then add 300 ml of ethanol in portions, stir for 10 min, the product will precipitate as flocculent, remove the supernatant, transfer the precipitate to a 50 ml centrifuge tube, and centrifuge at 9000 rpm for 20 min; (4) The supernatant was removed, deionized water was added to 15 mL, and the mixture was shaken evenly. 10 mL of ethyl acetate was added, and then 50 mL of ethanol was added and shaken evenly. The mixture was centrifuged at 9000 rpm for 20 min, the supernatant was removed, and the mixture was mixed to obtain a nanosilver paste (A4). The SEM photograph of the silver particles is shown in FIG. Figure 7 The particle size is <720nm. The SEM photo of the silver film obtained after sintering is shown in Figure 8 shown.

[0084] Example 5 A method for preparing a low-temperature sintered conductive silver paste comprises the following steps: (1) Take 20g AgNO3 (118mmol) and dissolve it in 20g deionized water to prepare a silver nitrate solution. Add 50g deionized water into a conical flask, then add 3g PAA (MW 3000) and 1g PAA (MW 20,000) in sequence, start stirring, and drop the silver nitrate solution into the conical flask. Finally, pour 14.4g (236mmol) ethanolamine into the conical flask at a faster rate and stir at 300r / min for 2h. (2) Heat and stir on a hot plate at 120°C for 2 h, then pour 8.8 g (59 mmol) of triethanolamine into the conical flask and continue heating and stirring for 2 h; (3) Cool to room temperature, add 100 ml of ethyl acetate, then add 300 ml of ethanol in portions, stir for 10 min, the product will precipitate as flocculent, remove the supernatant, transfer the precipitate to a 50 ml centrifuge tube, and centrifuge at 9000 rpm for 20 min; (4) The supernatant was removed, deionized water was added to 15 mL, and the mixture was shaken evenly. 10 mL of ethyl acetate was added, and then 50 mL of ethanol was added and shaken evenly. The mixture was centrifuged at 9000 rpm for 20 min, the supernatant was removed, and the mixture was mixed to obtain a nanosilver paste (A5). The SEM photograph of the silver particles is shown in FIG. Fig. 9 The particle size is <400nm. The SEM photo of the silver film obtained after sintering is shown in FIG. Fig.10 shown.

[0085] Example 6 A method for preparing a low-temperature sintered conductive silver paste comprises the following steps: (1) Take 20g AgNO3 (118mmol) and dissolve it in 20g deionized water to prepare a silver nitrate solution. Add 50g deionized water into a conical flask, then add 3g PAA (MW 3000) and 1g PAA (MW 20,000) in sequence, start stirring, and drop the silver nitrate solution into the conical flask. Finally, pour 14.4g (236mmol) ethanolamine into the conical flask at a faster rate and stir at 300r / min for 2h. (2) Heat and stir on a hot plate at 120°C for 2 h, then pour 7.8 g (59 mmol) of diisopropanolamine into the conical flask and continue heating and stirring for 2 h; (3) Cool to room temperature, add 100 ml of ethyl acetate, then add 300 ml of ethanol in portions, stir for 10 min, the product will precipitate as flocculent, remove the supernatant, transfer the precipitate to a 50 ml centrifuge tube, and centrifuge at 9000 rpm for 20 min; (4) The supernatant was removed, deionized water was added to 15 mL, and the mixture was shaken evenly. 10 mL of ethyl acetate was added, and then 50 mL of ethanol was added and shaken evenly. The mixture was centrifuged at 9000 rpm for 20 min, the supernatant was removed, and the mixture was mixed to obtain a nanosilver paste (A5). The SEM photograph of the silver particles is shown in FIG. Fig.11 The particle size is <400nm. The SEM photo of the silver film obtained after sintering is shown in FIG. Fig.12 shown.

[0086] Embodiment 7:

Preparation of silver paste

[0087]

Synthesis of cross-linked products of ligand and PAA

Preparation of low temperature conductive paste

[0088] Embodiment 8:

Preparation of silver paste

[0089]

Synthesis of cross-linked products of ligand and PAA

Preparation of low temperature conductive paste

[0090] Embodiment 9:

Preparation of silver paste

[0091]

Synthesis of cross-linked products of ligand and PAA

Preparation of low temperature conductive paste

[0092] Embodiment 10:

Preparation of silver paste

[0093]

Synthesis of cross-linked products of ligand and PAA

[0094]

Preparation of low temperature conductive paste

[0095] Embodiment 11:

Preparation of silver paste

[0096]

Synthesis of cross-linked products of ligand and PAA

[0097]

Preparation of low temperature conductive paste

[0098] Embodiment 12:

Preparation of silver paste

[0099]

Synthesis of cross-linked products of ligand and PAA

[0100]

Preparation of low temperature conductive paste

[0101] Embodiment 13:

Preparation of silver paste

[0102]

Synthesis of cross-linked products of ligand and PAA

[0103]

Preparation of low temperature conductive paste

[0104] Embodiment 14:

Preparation of silver paste

[0105]

Synthesis of cross-linked products of ligand and PAA

[0106]

Preparation of low temperature conductive paste

[0107] Embodiment 15:

Preparation of silver paste

[0108]

Synthesis of cross-linked products of ligand and PAA

[0109]

Preparation of low temperature conductive paste

[0110] Comparative Example 1:

Preparation of silver paste

[0111] Comparative Example 2:

Preparation of silver paste

[0112] Comparative Example 3 A method for preparing a low-temperature sintered conductive silver paste comprises the following steps: (1) Take 20g AgNO3 (118mmol), dissolve it in 20g deionized water to prepare a silver nitrate solution, add 50g deionized water into a conical flask, then add 4g PAA (MW 800) in sequence, start stirring, add the silver nitrate solution dropwise into the conical flask, and finally pour 14.4g (236mmol) ethanolamine into the conical flask at a faster rate, and stir at 300r / min for 2h; (2) Heat and stir on a hot plate at 120°C for 2 h, then pour 6.2 g (59 mmol) of diethanolamine into the conical flask and continue heating and stirring for 2 h; (3) Cool to room temperature, add 100 ml of ethyl acetate, then add 300 ml of ethanol in portions, stir for 10 min, the product will precipitate as flocculent, remove the supernatant, transfer the precipitate to a 50 ml centrifuge tube, and centrifuge at 9000 rpm for 20 min; (4) The supernatant was removed, deionized water was added to 15 mL, and the mixture was shaken evenly. 10 mL of ethyl acetate was added, and then 50 mL of ethanol was added and shaken evenly. The mixture was centrifuged at 9000 rpm for 20 min, and the supernatant was removed and mixed to obtain a nanosilver paste (D3). The SEM photograph of the nanosilver paste is shown in FIG. Fig.29 The particle size is >1 μm. The SEM image of the silver film obtained after sintering is shown in Fig.30 shown.

[0113] Comparative Example 4 A method for preparing a low-temperature sintered conductive silver paste comprises the following steps: (1) Take 20g AgNO3 (118mmol), dissolve it in 20g deionized water to prepare a silver nitrate solution, add 50g deionized water into a conical flask, then add 4g PAA (MW 250,000) in sequence, start stirring, add the silver nitrate solution dropwise into the conical flask, and finally pour 14.4g (236mmol) ethanolamine into the conical flask at a faster rate, and stir at 300r / min for 2h; (2) Heat and stir on a hot plate at 120°C for 2 h, then pour 6.2 g (59 mmol) of diethanolamine into the conical flask and continue heating and stirring for 2 h; (3) Cool to room temperature, add 100 ml of ethyl acetate, then add 300 ml of ethanol in portions, stir for 10 min, the product will precipitate as flocculent, remove the supernatant, transfer the precipitate to a 50 ml centrifuge tube, and centrifuge at 9000 rpm for 20 min; (4) The supernatant was removed, deionized water was added to 15 mL, and the mixture was shaken evenly. 10 mL of ethyl acetate was added, and 50 mL of ethanol was added and shaken evenly. The mixture was centrifuged at 9000 rpm for 20 min, the supernatant was removed, and the mixture was mixed to obtain a nanosilver paste (D4). The SEM photograph of the nanosilver paste is shown in FIG. Fig.31 The particle size is <150nm. The SEM photo of the silver film obtained after sintering is shown in Fig.32 shown.

[0114] Comparative Example 5

Preparation of silver paste

[0115]

Synthesis of cross-linked products of ligand and PAA

[0116]

Preparation of low temperature conductive paste

[0117] Comparative Example 6

Preparation of silver paste

[0118]

Synthesis of cross-linked products of ligand and PAA

[0119]

Preparation of low temperature conductive paste

[0120] Comparative Example 7

Preparation of silver paste

[0121]

Synthesis of cross-linked products of ligand and PAA

[0122]

Preparation of low temperature conductive paste

[0123] Comparative Example 8

Preparation of silver paste

[0124]

Synthesis of cross-linked products of ligand and PAA

[0125]

Preparation of low temperature conductive paste

[0126]

Performance test

[0127] The specific method is: ① Take a small amount of silver paste and dilute it in deionized water or organic solvent at a ratio of 1:1000; ② Disperse the dilution fully, pipette a small amount and add it to the surface of the carrier and heat to remove excess solvent; ③ Prepare the sample and spray gold, then send the sample for observation to obtain the size and morphology image information of the silver nanoparticles.

[0128] (2) Resistivity test: The resistivity of silver paste and low-temperature conductive paste with added resin was tested using a Ruike Weiye FT-340 four-probe square resistance tester.

[0129] The specific method is as follows: ① The prepared silver paste and low-temperature conductive paste are scraped onto the glass original plate through a coating machine, and sintered at 200°C in air for 60 minutes to obtain a conductive silver film; ② The thickness of the silver film sample after sintering is measured with the help of a step meter; ③ The corresponding parameters are set in the square resistance meter, and the four-probe probe is adjusted to press down vertically above the sample to be tested and touch lightly; ④ After the reading is stable, the square resistance, resistivity and other data are recorded.

[0130] (3) Hundred-grid test ① The prepared low-temperature conductive slurry is coated on the original glass plate by a coating machine, and sintered at 200°C in air for 60 minutes to obtain a conductive silver film; ② Using ASTM D3359-2017 as the test standard, use a grid knife to cut the surface of the test piece at a cutting speed of 20-50mm / s; ③ Rotate the test piece 90° and repeat the above operation on the cut to form a grid pattern; ④ Use a soft brush to brush the diagonal lines on both sides of the grid pattern, brushing lightly 5 times each; ⑤Use 3M 600-1PK test tape to perform peel test and evaluate the bonding performance of the material.

[0131] The test results of the low temperature sintering conductive silver paste prepared in Examples 1 to 15 and Comparative Examples 1 to 8 are shown in Tables 1 to 2 below: Table 1 a:σ a is the conductivity of the conductive silver film after sintering of the corresponding slurry; b: σ Ag is the electrical conductivity of silver metal (value is 63 kS / mm); σ a / σ Ag It is the ratio of the conductivity of the conductive silver film to the conductivity of pure silver.

[0132] Table 2 a:σ a is the conductivity of the conductive silver film after sintering of the corresponding slurry; b: σ Ag is the electrical conductivity of silver metal (value is 63 kS / mm); σ a / σ Ag It is the ratio of the conductivity of the conductive silver film to the conductivity of pure silver.

[0133]

Result Analysis

[0134] It can be seen from Comparative Example 1 that due to the lack of addition of polyol amine in Comparative Example 1, the adhesion of the silver paste finally prepared is weak, and thus it cannot pass the adhesion test.

[0135] It can be seen from Comparative Example 2 that since diethanolamine is used as a reducing agent in Comparative Example 2, diethanolamine is likely to simultaneously produce a cross-linking reaction with the ligand during the process of reducing silver ions to form silver nanoparticles. Therefore, the obtained product will be a complex of silver nanoparticles-ligands-polyol amines, and the ligands will simultaneously cross-link with the silver nanoparticles and the polyol amines. Since the silver nanoparticles-ligands-polyol amine complex obtained in this way is difficult to decompose at low temperatures, the sintering effect of the conductive silver paste at low temperatures is poor. Under normal conditions, it can only be sintered at a temperature above 300°C to obtain a higher conductivity.

[0136] It can be seen from Comparative Example 3 that since the molecular weight of the ligand used in Comparative Example 3 is relatively low, it cannot provide sufficient adhesion after being cross-linked with the polyol amine, resulting in it failing to pass the adhesion test.

[0137] It can be seen from Comparative Example 4 that since the molecular weight of the ligand used in Comparative Example 4 is relatively high, although it has good bonding properties, it greatly reduces the conductivity of the silver paste.

[0138] It can be seen from Comparative Example 5 that since the content of the cross-linked product of the ligand and PAA used in Comparative Example 5 is relatively low, it cannot provide sufficient adhesion for the conductive silver paste.

[0139] It can be seen from Comparative Example 6 that since the content of the cross-linked product of the ligand and PAA used in Comparative Example 6 is too high, although its bonding performance is good, it seriously affects the conductive performance of the conductive silver paste.

[0140] It can be seen from Comparative Example 7 that due to the excessively high content of the diluent in Comparative Example 7, its overall performance is inferior to that of Examples 1 to 14.

[0141] It can be seen from Comparative Example 8 that since the content of the diluent in Comparative Example 8 is too low, it is difficult to disperse the components evenly, and it cannot be applied to 3D printing scenarios of three-dimensional structures below 10 μm.

[0142] In summary, the silver nanoparticles of the low-temperature sintered conductive silver paste of the present invention are synthesized by a water-phase synthesis method during the preparation process, and the cross-linked product of polyol amine and ligand is selected as a binder. Since the cross-linked product is homologous to the ligand, it can provide a certain degree of adhesion to the paste, and will not have dispersion problems caused by differences in compatibility. Therefore, it can ensure that the conductivity is ≥6.3kS / mm after low-temperature sintering at 150-200℃, while ensuring that the adhesion of the silver paste to the substrate is ≥4B, so that it can be applied to 3D printing scenarios of three-dimensional structures below 10μm.

Claims

1. A low temperature sintering conductive silver paste, characterized in that: including silver nanoparticles; The silver nanoparticles have ligands chemically bonded to their surfaces; Also included are ligand-polyol amine cross-linked products formed by chemical bonding of the ligand and the polyol amine.

2. A low temperature sintering conductive silver paste according to claim 1, characterized in that: The silver paste also includes a diluent.

3. A low temperature sintering conductive silver paste according to claim 2, characterized in that: The silver paste comprises the following components by mass percentage: 65-95% of silver nanoparticles, 2-10% of ligand-polyol amine cross-linked product and 3-25% of diluent.

4. A low temperature sintering conductive silver paste according to any one of claims 1 to 3, characterized in that: The ligand is an unsaturated organic acid polymer with the general structural formula shown in the following formulas (Ⅰ), (Ⅱ), and (Ⅲ); Formula (I): Formula (II): Formula (III): Wherein: R1, R2, R3 are alkyl or H.

5. The low temperature sintering conductive silver paste according to claim 4, characterized in that: The ligand is any one or more of polyacrylic acid, polymethacrylic acid, polymaleic acid, maleic acid-acrylic acid copolymer and homologues thereof.

6. The low temperature sintering conductive silver paste according to claim 5, characterized in that: The ligand is polyacrylic acid with a molecular weight between 3000 and 200000.

7. A low temperature sintering conductive silver paste according to claim 2 or 3, characterized in that: The diluent is a solvent with carbon number / hydroxyl group ≤4 and hydroxyl number ≥2.

8. The low temperature sintering conductive silver paste according to claim 7, characterized in that: The diluent includes any one or more combinations of water, ethylene glycol, glycerol, 1,4-butanediol, isoprene glycol, and trimethylolpropane.

9. A low temperature sintering conductive silver paste according to any one of claims 1 to 3, characterized in that: The polyol amine has a general chemical formula of (CH2) a (OH) b NH secondary alcohol amine or chemical formula (CH2) a (OH) b Any one or more combinations of tertiary alcohol amines of N; Among them: 2≤a / b≤6, 2≤b≤6.

10. The low temperature sintering conductive silver paste according to claim 9, characterized in that: The polyol amine is any one or more combinations of diethanolamine, triethanolamine, diisopropanolamine and triisopropanolamine.

11. A method for preparing a low temperature sintered conductive silver paste as claimed in any one of claims 1 to 10, characterized in that: The following steps are involved: (S.1) mixing a silver salt solution with a ligand solution, and using a monohydric alcohol amine as a reducing agent to react to obtain a liquid phase system including silver nanoparticles with surface chemically bonded ligands and free ligands; (S.2a) adding a polyol amine to the liquid phase system obtained in step (S.1) to allow the free ligand to undergo a cross-linking reaction with the polyol amine to obtain a ligand-polyol amine cross-linked product, and finally purifying the entire system using a purification solvent to obtain the low-temperature sintering conductive silver paste; or, (S.2b) purifying the liquid phase system obtained in step (S.1) with a purification solvent to obtain silver nanoparticles with surface chemically bonded ligands, mixing the ligands with polyol amines and heating them to form ligand-polyol amine crosslinked products, and uniformly mixing the silver nanoparticles with surface chemically bonded ligands and the ligand-polyol amine crosslinked products to obtain the low-temperature sintering conductive silver paste; (S.3) adding a diluent to the low temperature sintering conductive silver paste to adjust the viscosity of the low temperature sintering conductive silver paste.

12. The method according to claim 11, characterized in that The monohydric alcohol amine has a general formula of OH-X-NH2, wherein X is an alkane chain with 2≤carbon number≤6.

13. The method according to claim 11, characterized in that The purification solvent includes a good solvent containing a hydroxyl group or a carbonyl group, and a sub-good solvent containing an ester group.

14. The method according to claim 13, characterized in that The good solvent is any one or more of methanol, ethanol and acetone; The sub-good solvent is any one or more combinations of ethyl acetate, propyl acetate and butyl acetate.

15. Application of the low-temperature sintered conductive silver paste as claimed in any one of claims 1 to 10 or the low-temperature sintered conductive silver paste prepared by the method as claimed in any one of claims 11 to 14 in high-precision direct writing 3D printing of 10 μm and below, precision optics, micro-nano chips, photovoltaics or printed electronics.

Citation Information

Cited By

  • Low-temperature pressureless sintering type silver paste and preparation method and application thereof

    CN119763897A