Preparation method of low-resistance conductive paste, carbon-coated aluminum foil and preparation method of carbon-coated aluminum foil

By applying a water-resistant and wear-resistant low-resistance carbon coating layer on the aluminum foil, the problem of carbon-coated aluminum foil swelling in aqueous sodium ion batteries is solved, the water resistance and conductivity of the battery are improved, and the stability of the battery performance is ensured.

CN119028658APending Publication Date: 2024-11-26GUANGDONG LEARY NEW MATERIAL TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411115902.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing carbon-coated aluminum foils are prone to swell when exposed to water, resulting in an increase in the internal resistance of lithium-ion batteries and cannot meet the conditions for use of aqueous sodium ion batteries.

Method used

Using a preparation method of low resistance conductive paste, by drying resin A and nano-scale conductive materials in a protective atmosphere, adding chain extenders and additives to form water-resistant and wear-resistant water-based polyurethane emulsions, and with carbon-based conductive materials Mixed, a water-resistant and wear-resistant carbon coating layer is formed on the aluminum foil by microgravure coating technology.

Benefits of technology

It effectively improves the water resistance and conductivity of carbon-coated aluminum foil, solves the problem of water swelling of the carbon-coated layer, and ensures the stability of battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993607530000051
    Figure BDA0004993607530000051
  • Figure BDA0004993607530000081
    Figure BDA0004993607530000081
  • Figure BDA0004993607530000131
    Figure BDA0004993607530000131
Patent Text Reader

Abstract

The invention discloses a preparation method of low-resistance conductive paste, a carbon-coated aluminum foil and a preparation method of the carbon-coated aluminum foil. Comprising the following steps: S1, drying resin A, cooling, adding resin B and a nanoscale conductive material, and stirring to obtain a mixed solution; s2, cooling the mixed solution prepared in the step S1, adding a chain extender, stirring, cooling to normal temperature, and adding water to prepare a polyurethane emulsion; s3, adding an auxiliary agent into the polyurethane emulsion prepared in the step S2, and stirring to prepare a waterborne polyurethane emulsion; s4, mixing a carbon conductive material and an ethanol water solution, stirring, adding the waterborne polyurethane emulsion prepared in the step S3, and grinding to prepare conductive slurry; the resin A is polyol; and the resin B is aliphatic diisocyanate. The carbon-coated aluminum foil with excellent performance can be prepared through the conductive slurry, and the problem that an existing carbon-coated aluminum foil is prone to swelling when encountering water is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon-coated aluminum foil, and in particular to a method for preparing a low-resistance conductive slurry, a carbon-coated aluminum foil and a preparation method thereof. Background Art

[0002] Under the general background of "carbon neutrality", lithium-ion batteries have been successfully commercialized as power sources for electronic devices and electric vehicles due to their high energy density and long cycle life. However, due to the scarcity and uneven distribution of lithium and cobalt resources, lithium-ion batteries cannot be a permanent solution, which has promoted the development of new rechargeable battery technologies.

[0003] As a potential post-lithium-ion battery technology, aqueous sodium-ion batteries have attracted great attention due to their low cost, wide geographical distribution of sodium resources, high safety, and environmental friendliness. Although the inherent advantages of aqueous sodium-ion batteries, such as wide temperature range and excellent rate performance, have proven their value in large-scale energy storage systems, the relatively low energy density of aqueous sodium ions limits their ability to completely replace lithium-ion batteries.

[0004] Carbon-coated aluminum foil is widely used in lithium-ion batteries. It can provide more lithium storage space for lithium-ion batteries, thereby achieving the effect of improving energy density. This product is also suitable for aqueous sodium-ion batteries to improve the energy density of sodium-ion batteries. However, most of the carbon-coated aluminum foils in the prior art use water-based acrylic resin to prepare the slurry and form a carbon coating layer on the aluminum foil. The carbon coating layer prepared by this method easily causes swelling between the aluminum foil and the carbon coating layer when it comes into contact with water, which increases the internal resistance of the battery and cannot meet the use conditions of sodium-ion batteries in aqueous electrolytes. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a low-resistance conductive slurry, which can be used to prepare a conductive slurry with excellent water resistance, wear resistance and conductivity. A carbon-coated aluminum foil with excellent performance can be prepared through the conductive slurry, solving the problem that the existing carbon-coated aluminum foil is easy to swell when exposed to water.

[0006] Another object of the present invention is to provide a method for preparing a low-resistance carbon-coated aluminum foil, which can prepare a carbon-coated aluminum foil with excellent water resistance, wear resistance and conductivity, and solve the problem that the existing carbon-coated aluminum foil is easy to swell when exposed to water.

[0007] Another object of the present invention is to provide a low-resistance carbon-coated aluminum foil to solve the problem that the existing carbon-coated aluminum foil is easily swollen when exposed to water.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] A method for preparing a low-resistance conductive paste comprises the following steps:

[0010] S1. Drying resin A in a protective gas atmosphere, adding resin B and nano-scale conductive material after cooling, and stirring to obtain a mixed solution;

[0011] S2, after the mixed solution obtained in step S1 is cooled, a chain extender is added and stirred, the mixture is cooled to room temperature, and water is added to obtain a polyurethane emulsion;

[0012] S3, adding an auxiliary agent to the polyurethane emulsion prepared in step S2 and stirring to prepare an aqueous polyurethane emulsion;

[0013] S4, mixing a carbon-based conductive material and an ethanol aqueous solution, stirring, adding the aqueous polyurethane emulsion obtained in step S3, and grinding to obtain a conductive slurry;

[0014] The resin A is a polyol; and the resin B is an aliphatic diisocyanate.

[0015] Furthermore, the resin A is one or more of alkyd resin, polyester resin, polyether resin and acrylic resin;

[0016] The resin B contains an R group, and the R group is one or more of hexamethylene, xylylene, isophorone, dicyclohexylmethane, tetramethyl-m-xylylene, diphenylmethane, and dicyclohexylmethane.

[0017] Furthermore, the molar ratio of resin A:resin B is 1:(1.85-2.5).

[0018] Furthermore, the number average molecular weight of the resin A is 1000-3000 g / mol;

[0019] The number average molecular weight of the polyurethane emulsion is 320,000-600,000 g / mol.

[0020] Furthermore, the nano-scale conductive material accounts for 0.01-0.1% of the total weight of the conductive paste.

[0021] Further, the conductive paste includes 5-8 parts of carbon-based conductive material, 10-18 parts of waterborne polyurethane emulsion, and 74-82 parts of ethanol aqueous solution, calculated by weight;

[0022] The solid content of waterborne polyurethane emulsion is 45-55%.

[0023] Furthermore, the nanoscale conductive material is one or more of carbon nanotubes, multi-walled carbon nanotubes, graphene, and graphene oxide;

[0024] The carbon-based conductive material is one or more of amorphous carbon, graphene, conductive graphite, carbon nanotubes, and SP.

[0025] Furthermore, the chain extender is 2,2-bis(hydroxymethyl)propionic acid.

[0026] A method for preparing a low-resistance carbon-coated aluminum foil, wherein the conductive paste is prepared by the method for preparing a low-resistance conductive paste;

[0027] The conductive slurry is coated on the aluminum foil and dried to obtain the low-resistance carbon-coated aluminum foil.

[0028] A low-resistance carbon-coated aluminum foil is prepared by the method for preparing the low-resistance carbon-coated aluminum foil.

[0029] Compared with the prior art, the technical solution proposed in the present invention can have the following beneficial effects:

[0030] 1. The large amount of hydroxyl groups (-OH) in resin A react quickly with the isocyanate structure (-NCO) of resin B to form a prepolymer, which makes the entire reaction process more efficient and more controllable. Among them, the HNCO-R-CONH structure of the prepolymer is water-resistant, and the aliphatic resin B is also hydrophobic, which effectively improves the water resistance of the conductive paste prepared in this scheme;

[0031] 2. A conductive slurry is coated on aluminum foil using micro-gravure coating technology to prepare a low-resistance carbon-coated aluminum foil for aqueous sodium-ion batteries that is water-resistant, wear-resistant, and has good conductivity. This solves the problem that the traditional carbon-coated layer easily swells with aluminum when it comes into contact with water, thereby increasing the internal resistance of the battery. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further explained below in conjunction with specific implementation methods.

[0033] The invention provides a method for preparing a low-resistance conductive slurry, a carbon-coated aluminum foil and a preparation method thereof.

[0034] A method for preparing a low-resistance conductive paste comprises the following steps:

[0035] S1. Drying resin A in a protective gas atmosphere, adding resin B and nano-scale conductive material after cooling, and stirring to obtain a mixed solution;

[0036] S2, after the mixed solution obtained in step S1 is cooled, a chain extender is added and stirred, the mixture is cooled to room temperature, and water is added to obtain a polyurethane emulsion;

[0037] S3, adding an auxiliary agent to the polyurethane emulsion prepared in step S2 and stirring to prepare an aqueous polyurethane emulsion;

[0038] S4, mixing a carbon-based conductive material and an ethanol aqueous solution, stirring, adding the aqueous polyurethane emulsion obtained in step S3, and grinding to obtain a conductive slurry;

[0039] The resin A is a polyol; and the resin B is an aliphatic diisocyanate.

[0040] In step S1, resin A is dried under a protective gas atmosphere to completely remove the moisture in resin A, ensuring that a large amount of hydroxyl groups (-OH) in resin A react quickly with resin B with an isocyanate structure (-NCO) to form a prepolymer, making the entire reaction process more efficient and more controllable. Among them, the HNCO-R-CONH structure of the prepolymer is water-resistant, and the aliphatic resin B is also hydrophobic, which effectively improves the water resistance of the conductive paste of this scheme.

[0041] Nano-scale conductive materials are prone to agglomeration. When synthesizing polyurethane particles, the R group in resin B can play a steric hindrance role and can have a good dispersion effect on nano-materials. In addition, during the synthesis of polyurethane, since there are more hydrogen bonds in the polyurethane particles, it is conducive to the adsorption of nano-scale conductive materials, so that the surface of the nano-scale conductive material is functionalized, and then the groups in the polyurethane particles can be grafted on the surface of the nano-scale conductive material, further enhancing the dispersion effect of the nano-scale conductive material, so that the final synthesized polyurethane emulsion can further improve its water resistance, wear resistance and conductivity.

[0042] The chain extender contains a carboxylic acid group (-COOH), which can ensure that the final synthesized polyurethane emulsion can form an aqueous polyurethane emulsion in water. In addition, the chain extender can accelerate the polymerization reaction, increase the molecular weight of the polyurethane resin and the degree of cross-linking of the resin.

[0043] The additives are wetting agent and defoamer, accounting for 0.01%-0.2% of the total weight respectively. The defoamer can quickly and effectively eliminate the foam and bubbles generated during the reaction and improve the quality of the conductive paste. The wetting agent not only helps the polyurethane to mix better with the carbon-based conductive material during the processing, but also allows the polyurethane particles to be evenly dispersed in the ethanol aqueous solution to improve the uniformity and consistency of the conductive paste.

[0044] Furthermore, the resin A is one or more of alkyd resin, polyester resin, polyether resin and acrylic resin;

[0045] The resin B contains an R group, and the R group is one or more of hexamethylene, xylylene, isophorone, dicyclohexylmethane, tetramethyl-m-xylylene, diphenylmethane, and dicyclohexylmethane.

[0046] The various resins A selected are all polyol structures and have a large number of hydroxyl groups (-OH). Aliphatic diisocyanates not only provide isocyanate groups (-NCO), but also R groups. Among them, the isocyanate groups in resin B react with the hydroxyl groups in resin A to form a prepolymer with a HNCO-R-CONH structure. The reaction formula is as follows:

[0047]

[0048] The HNCO-R-CONH structure is water-resistant and can improve the water resistance of the carbon coating layer.

[0049] The R group (hexamethylene, xylylene, isophorone, dicyclohexylmethane, tetramethyl-m-xylylene, diphenylmethane, dicyclohexylmethane) in resin B can provide a good steric hindrance, which is conducive to the dispersion of nano-scale carbon-based electrical materials; and the R group is hydrophobic, which further improves the water resistance of the carbon coating. Therefore, resin B is preferably one or more of hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, tetramethyl-m-xylylene diisocyanate, diphenylmethane diisocyanate, and dicyclohexylmethane diisocyanate.

[0050] Furthermore, the molar ratio of resin A:resin B is 1:(1.85-2.5).

[0051] This solution controls the molecular weight of polyurethane by limiting the molar ratio of resin A: resin B, affects the ratio of isocyanate groups to hydroxyl groups in the polyurethane emulsion, and thus affects the water resistance of the carbon coating layer. When the content of resin B increases, that is, when the amount of isocyanate groups is large, polyurethane will produce more urea segments, that is, HNCO-R-CONH structures, etc. during emulsification, which reduces the water absorption rate of polyurethane and enhances water resistance.

[0052] However, when the content of resin B exceeds this range, the R group of the rigid segment increases, the hydrogen bonding and cross-linking effects are enhanced, which will limit the movement between molecules. Therefore, the polyurethane produced will be relatively brittle after curing, making the wear resistance of the carbon coating layer poor.

[0053] Furthermore, the number average molecular weight of the resin A is 1000-3000 g / mol;

[0054] The number average molecular weight of the polyurethane emulsion is 320,000-600,000 g / mol.

[0055] Since the resin A used in this scheme is a macromolecular structure, the resin A with a large molecular weight has poor fluidity and a long reaction time, which is not conducive to the connection of resin B to resin A. When the molecular weight of resin A is low, the viscosity of the prepared polyurethane emulsion is low and the film-forming property of the product is poor. Therefore, this scheme limits the number average molecular weight of resin A to ensure that the carbon coating layer has good water resistance, wear resistance and conductivity.

[0056] In addition, according to the number average molecular weight of resin A and the molar ratio of resin A:resin B, the number average molecular weight of the polyurethane emulsion can also be controlled within a specific range, which can ensure that the finished carbon-coated aluminum foil has water resistance, wear resistance and conductivity. If the number average molecular weight of the polyurethane emulsion is too large, the dispersibility of the polyurethane particles in the ethanol aqueous solution may be affected, making it difficult to disperse evenly, which seriously affects the performance of the carbon coating layer.

[0057] Furthermore, the nano-scale conductive material accounts for 0.01-0.1% of the total weight of the conductive paste.

[0058] Nano-scale conductive materials are prone to agglomeration. When synthesizing polyurethane, the groups in polyurethane can be grafted on the surface of nano-scale conductive materials, which is conducive to the dispersion of nano-scale conductive materials and further improves the water resistance and conductivity of polyurethane. However, when the addition of nano-scale conductive materials exceeds this range, the viscosity of polyurethane increases, which is not conducive to production.

[0059] Further, the conductive paste includes 5-8 parts of carbon-based conductive material, 10-18 parts of waterborne polyurethane emulsion, and 74-82 parts of ethanol aqueous solution, calculated by weight;

[0060] The solid content of waterborne polyurethane emulsion is 45-55%.

[0061] In this solution, the solid content of polyurethane is limited so that the content ratio of polyurethane particles to carbon-based conductive material is approximately 1:1, to ensure the conductive performance of the conductive paste. If the content of polyurethane is too much, the conductive performance of the carbon coating will be affected; if the resin is too little, the carbon-based conductive material will not be firmly bonded and will easily fall off, which will also affect the conductive performance of the carbon coating.

[0062] In this solution, the content of ethanol aqueous solution is relatively high, which can increase the leveling property of the conductive paste and the dispersibility of the conductive material to the carbon-based conductive material.

[0063] It is worth noting that the weight ratio of deionized water to ethanol in the ethanol aqueous solution is (8-9): (1-2). When the amount of ethanol in the ethanol aqueous solution exceeds the specified range, the polyurethane emulsion in the system will precipitate into the alcohol, causing the conductive paste to fail and being unfavorable for film formation.

[0064] Furthermore, the nanoscale conductive material is one or more of carbon nanotubes, multi-walled carbon nanotubes, graphene, and graphene oxide;

[0065] The carbon-based conductive material is one or more of amorphous carbon, graphene, conductive graphite, carbon nanotubes, and SP.

[0066] Nano-scale conductive materials have strong conductivity and can improve the dielectric constant of polyurethane solutions. At the same time, the groups in polyurethane particles can be grafted on the surface of nano-scale conductive materials, thereby improving the dispersion of nano-scale conductive materials in polyurethane solutions, thereby improving the water resistance of conductive pastes.

[0067] The carbon-based conductive material is evenly distributed in the conductive paste, which can provide a higher specific surface area and further enhance the conductive properties of the conductive paste. In addition, the combination of carbon-based conductive materials and polyurethane solution may help improve the adhesion between the carbon coating layer and the aluminum foil, solving the problem that the existing aluminum foil and the carbon coating layer are easy to swell when exposed to water. The more urea segments and aliphatic group structural characteristics in the polyurethane are used to enhance the carbon coating layer's resistance to swelling in water, ensuring the stability of the battery performance.

[0068] Furthermore, the chain extender is 2,2-bis(hydroxymethyl)propionic acid. It is worth noting that 2,2-bis(hydroxymethyl)propionic acid contains a hydrophilic carboxylic acid group (-COOH). The chain extender containing a carboxylic acid group reacts at both ends of the polyurethane particles, and the reaction formula is as follows:

[0069]

[0070] The main part of the final synthesized polyurethane particles is hydrophobic, and the carboxylic acid groups at both ends are hydrophilic, which ensures that the final synthesized resin can form an emulsion in water. The second function of the chain extender is to speed up the reaction, increase the molecular weight of the prepolymer, and reduce the activation energy of the reaction.

[0071] A method for preparing a low-resistance carbon-coated aluminum foil comprises the following steps:

[0072] A conductive paste is prepared by a method for preparing a low-resistance conductive paste;

[0073] The conductive slurry is coated on the aluminum foil and dried to obtain the low-resistance carbon-coated aluminum foil.

[0074] The nano-scale conductive material in the conductive slurry has strong conductive properties and can make the surface of the low-resistance carbon-coated aluminum foil prepared by this scheme smooth and wear-resistant, thereby improving water resistance.

[0075] In this scheme, a conductive slurry is coated on the aluminum foil using micro-gravure coating technology to prepare a low-resistance carbon-coated aluminum foil for aqueous sodium ion batteries that is water-resistant, wear-resistant, and has good conductivity. This solves the problem that the traditional carbon-coated layer easily swells with aluminum when it comes into contact with water, thereby increasing the internal resistance of the battery.

[0076] A low-resistance carbon-coated aluminum foil, characterized in that it is prepared by a method for preparing a low-resistance carbon-coated aluminum foil.

[0077] The low-resistance carbon-coated aluminum foil prepared by the present invention has excellent water resistance, wear resistance and electrical conductivity, and can solve the problem that the existing aluminum foil and coating are easily swollen when exposed to water. The more urea segments and aliphatic group structural characteristics in the polyurethane are utilized to enhance the swelling resistance of the carbon coating layer to water, thereby ensuring the stability of the battery performance.

[0078] The present invention is further described below in conjunction with embodiments and comparative examples.

[0079] Example 1

[0080] S1. Dry 15 parts by weight of resin A in a nitrogen atmosphere for 1.5 hours and cool to 85°C; after cooling, add 30 parts by weight of resin B and 0.1 parts by weight of nano-conductive material and stir at a stirring speed of 600 r / min for 3 hours;

[0081] S2, after the mixed solution prepared in step S1 is cooled to 75° C., 1 part by weight of a chain extender is added and stirred at a stirring speed of 800 r / min for 2 h, and then cooled to room temperature, 53 parts by weight of deionized water are added to obtain a polyurethane emulsion, so that the solid content of the obtained polyurethane emulsion is 45%, and the number average molecular weight of the polyurethane emulsion is 320000 g / mol;

[0082] S3, adding an auxiliary agent to the polyurethane emulsion and stirring, the stirring speed is 100r / min, and the stirring time is 30min to obtain an aqueous polyurethane emulsion;

[0083] S4, deionized water and ethanol were mixed in a weight ratio of 8:2, stirring at a speed of 300 r / min for 15 min to obtain an ethanol aqueous solution. 6 parts by weight of carbon-based conductive material were added to 82 parts by weight of ethanol aqueous solution, stirring at a speed of 600 r / min for 30 min, and after stirring, 12 parts by weight of aqueous polyurethane emulsion were added, stirring at a speed of 600 r / min for 40 min, and grinding for 2 h to obtain a conductive paste;

[0084] S5. Coating slurry: Use micro-gravure coating technology to coat the conductive slurry on the aluminum foil, with a coating surface density of 1.2g / m 2 , and dried at 100°C for 1 min to form a carbon-coated aluminum foil.

[0085] Among them, resin A is a polyether resin with a number average molecular weight of 1797 g / mol; resin B is hexamethylene diisocyanate, the nano-scale conductive material is graphene oxide, the chain extender is 2,2-bis(hydroxymethyl)propionic acid (DMPA), the additives are 0.2 parts by weight of wetting agent BYK-348 and 0.01 parts by weight of defoaming agent BYK-025, and the carbon-based conductive material is a mixture of amorphous carbon and conductive graphite.

[0086] Example 2

[0087] S1. Dry 18 parts by weight of resin A in a helium atmosphere for 3 hours and cool to 90°C; after cooling, add 33 parts by weight of resin B and 0.05 parts by weight of nano-conductive material and stir at a stirring speed of 800 r / min for 3 hours;

[0088] S2, after the mixed solution prepared in step S1 is cooled to 85° C., 1 part by weight of a chain extender is added and stirred at a stirring speed of 800 r / min for 2 h, and then cooled to room temperature, 53 parts by weight of deionized water is added to obtain a polyurethane emulsion, so that the obtained polyurethane emulsion has a solid content of 55% and a number average molecular weight of 600,000 g / mol;

[0089] S3, adding an auxiliary agent to the polyurethane emulsion and stirring, the stirring speed is 200r / min, and the stirring time is 30min to obtain an aqueous polyurethane emulsion;

[0090] S4, deionized water and ethanol were mixed in a weight ratio of 9:1, the stirring speed was 500r / min, the stirring time was 15min, and an ethanol aqueous solution was prepared. 6 parts by weight of carbon-based conductive material was added to 82 parts by weight of ethanol aqueous solution, the stirring speed was 800r / min, the stirring time was 40min, and after stirring, 12 parts by weight of aqueous polyurethane emulsion was added, the stirring speed was 800r / min, the stirring time was 40min, and the conductive paste was prepared by grinding for 2h;

[0091] S5. Coating slurry: Use micro-gravure coating technology to coat the conductive slurry on the aluminum foil, with a coating surface density of 1.2g / m 2 , and dried at 100°C for 1 min to form a carbon-coated aluminum foil.

[0092] Among them, resin A is an alkyd resin with a number average molecular weight of 2973 g / mol; resin B is xylene diisocyanate, the nanoscale conductive material is carbon nanotubes, the chain extender is 2,2-bis(hydroxymethyl)propionic acid (DMPA), the additives are 0.2 parts by weight of wetting agent BYK-348 and 0.01 parts by weight of defoaming agent BYK-025, and the carbon-based conductive material is graphene.

[0093] Example 3

[0094] S1. Dry 20 parts by weight of resin A in a nitrogen atmosphere for 2 hours and cool to 87°C; after cooling, add 25 parts by weight of resin B and 0.08 parts by weight of nano-conductive material and stir at a stirring speed of 750 r / min for 3 hours;

[0095] S2, after the mixed solution prepared in step S1 is cooled to 80° C., 1 part by weight of a chain extender is added and stirred at a stirring speed of 700 r / min for 2 h, and then cooled to room temperature, 53 parts by weight of deionized water are added to obtain a polyurethane emulsion, so that the solid content of the obtained polyurethane emulsion is 50%, and the number average molecular weight of the polyurethane emulsion is 450000 g / mol;

[0096] S3, adding an auxiliary agent to the polyurethane emulsion and stirring, the stirring speed is 120r / min, and the stirring time is 30min to obtain an aqueous polyurethane emulsion;

[0097] S4, deionized water and ethanol were mixed in a weight ratio of 9:1, the stirring speed was 600r / min, the stirring time was 15min, and an ethanol aqueous solution was prepared. 6 parts by weight of carbon-based conductive material was added to 82 parts by weight of ethanol aqueous solution, the stirring speed was 700r / min, the stirring time was 40min, and after stirring, 12 parts by weight of aqueous polyurethane emulsion was added, the stirring speed was 700r / min, the stirring time was 40min, and the conductive paste was prepared by grinding for 2h;

[0098] S5. Coating slurry: Use micro-gravure coating technology to coat the conductive slurry on the aluminum foil, with a coating surface density of 1.2g / m 2 , and dried at 100°C for 1 min to form a carbon-coated aluminum foil.

[0099] Among them, resin A is acrylic resin with a number average molecular weight of 1150 g / mol; resin B is tetramethyl meta-xylylene diisocyanate, the nano-scale conductive material is graphene, the chain extender is 2,2-bis(hydroxymethyl)propionic acid (DMPA), the additives are 0.2 parts by weight of wetting agent BYK-348 and 0.01 parts by weight of defoaming agent BYK-025, and the carbon-based conductive material is carbon nanotubes.

[0100] Comparative Example 1:

[0101] This comparative example is basically the same as Example 1, except that the weight portion of the nano-scale conductive material is 0 portion.

[0102] Comparative Example 2:

[0103] This comparative example is substantially the same as Example 1, except that an equal weight portion of commercially available acrylic resin is used to replace the aqueous polyurethane solution.

[0104] Comparative Example 3:

[0105] This comparative example is basically the same as Example 1, except that the order of adding the nano-scale conductive materials is changed:

[0106] S1, drying 15 parts by weight of resin A in a nitrogen atmosphere for 1.5 hours, and cooling to 85°C; after cooling, adding 30 parts by weight of resin B and stirring at a stirring speed of 600 r / min for 3 hours;

[0107] S2, after the mixed solution prepared in step S1 is cooled to 75° C., 1 part by weight of a chain extender is added and stirred at a stirring speed of 800 r / min for 2 h, and then cooled to room temperature, 53 parts by weight of deionized water are added to obtain a polyurethane emulsion, so that the solid content of the obtained polyurethane emulsion is 45%, and the number average molecular weight of the polyurethane emulsion is 320000 g / mol;

[0108] S3, adding an auxiliary agent to the polyurethane emulsion and stirring, the stirring speed is 100r / min, and the stirring time is 30min to obtain an aqueous polyurethane emulsion;

[0109] S4, deionized water and ethanol were mixed at a weight ratio of 9:1, the stirring speed was 600r / min, the stirring time was 15min, and an ethanol aqueous solution was obtained. 6 parts by weight of carbon-based conductive material and 0.1 parts by weight of nano-scale conductive material were added to 82 parts by weight of ethanol aqueous solution, the stirring speed was 700r / min, the stirring time was 40min, and after stirring, 12 parts by weight of aqueous polyurethane emulsion was added, the stirring speed was 700r / min, the stirring time was 40min, and the conductive paste was obtained by grinding for 2h.

[0110] S5. Coating slurry: Use micro-gravure coating technology to coat the conductive slurry on the aluminum foil, with a coating surface density of 1.2g / m 2 , and dried at 100°C for 1 min to form a carbon-coated aluminum foil.

[0111] Among them, resin A is a polyether resin with a number average molecular weight of 1797 g / mol; resin B is hexamethylene diisocyanate, the nano-scale conductive material is graphene oxide, the chain extender is 2,2-bis(hydroxymethyl)propionic acid (DMPA), the additives are 0.2 parts by weight of wetting agent BYK-348 and 0.01 parts by weight of defoaming agent BYK-025, and the carbon-based conductive material is a mixture of amorphous carbon and conductive graphite.

[0112] According to the preparation methods of Examples 1-3 and Comparative Examples 1-3, a low-resistance carbon-coated aluminum foil was prepared and performance tested. The test results are shown in Table 1:

[0113] 1. Fully absorb the test solvent such as NMP or water with cotton, and wipe it back and forth 200 times in 2 seconds. If it is wiped more than 200 times and there is no leakage of the carbon coating base, it is qualified. If it is wiped less than 200 times and the base is leaked, record the maximum number of wipes and it is judged as unqualified.

[0114] 2. Electrode resistance test: Use Yuanneng electrode resistance meter to test, the test condition is 20MPa.

[0115] 3. Adhesion test: According to the GB / T 2790-1995 test method, use 15mm wide 3M tape to adhere to the carbon-coated aluminum foil, and use a tensile machine to peel it off at 180°.

[0116] Table 1 Test results of finished carbon-coated aluminum foils prepared in Examples 1-3 and Comparative Examples 1-3

[0117]

[0118]

[0119] Examples 1, 2, and 3 have different synthetic resin raw materials, and the results show a decrease in adhesion. It is speculated that this is because some sterically hindered groups in the synthetic resin (such as tetramethylbenzene) affect the adhesion of the resin, but all resins show good adhesion (>100N / m).

[0120] Moreover, the carbon-coated aluminum foils prepared in Examples 1, 2, and 3 have lower resistance values ​​and better electrical conductivity, meeting the use requirements of aqueous sodium ion batteries.

[0121] Compared with Comparative Example 1, Example 1 has better water resistance because the synthetic resin is water-based polyurethane, but the resistance of the electrode without adding functional nanomaterials is higher, and the conductivity of the carbon-coated aluminum foil is poor, which does not meet the use requirements of aqueous sodium ion batteries.

[0122] Comparative Example 2 is a mainstream commercial product acrylic resin. Acrylic resin has good metal adhesion performance, but there are more carboxylic acid groups (-COOH) in acrylic resin. The carboxylic acid groups are hydrophilic and cannot meet the water resistance requirements of aqueous sodium ion batteries. Therefore, it is very easy to be wiped off by water during water-resistant wiping. In addition, acrylic resin itself has a cross-linking effect, and acrylic resin itself is not conductive, which will increase resistance and does not meet the use requirements of aqueous sodium ion batteries.

[0123] Compared with Comparative Example 3, Example 1 adds nano-scale conductive materials together with ordinary carbon-based materials, so that the prepared water-based polyurethane has no conductive properties, the resistance of the carbon-coated aluminum foil is high, and the conductivity of the carbon-coated aluminum foil is poor, which does not meet the use requirements of aqueous sodium-ion batteries.

[0124] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.

Claims

1. A method for preparing a low-resistance conductive paste, characterized in that: The following steps are involved: S1. Drying resin A in a protective gas atmosphere, adding resin B and nano-scale conductive material after cooling, and stirring to obtain a mixed solution; S2, after the mixed solution obtained in step S1 is cooled, a chain extender is added and stirred, the mixture is cooled to room temperature, and water is added to obtain a polyurethane emulsion; S3, adding an auxiliary agent to the polyurethane emulsion prepared in step S2 and stirring to prepare an aqueous polyurethane emulsion; S4, mixing a carbon-based conductive material and an ethanol aqueous solution, stirring, adding the aqueous polyurethane emulsion obtained in step S3, and grinding to obtain a conductive slurry; The resin A is a polyol; and the resin B is an aliphatic diisocyanate.

2. The method for preparing a low-resistance conductive paste according to claim 1, characterized in that: The resin A is one or more of alkyd resin, polyester resin, polyether resin and acrylic resin; The resin B contains an R group, and the R group is one or more of hexamethylene, xylylene, isophorone, dicyclohexylmethane, tetramethyl-m-xylylene, diphenylmethane, and dicyclohexylmethane.

3. The method for preparing a conductive paste for low-resistance carbon-coated aluminum foil according to claim 1, characterized in that: The molar ratio of the resin A:resin B is 1:(1.85-2.5).

4. The method for preparing a low-resistance conductive paste according to claim 1, characterized in that: The number average molecular weight of the resin A is 1000-3000 g / mol; The number average molecular weight of the polyurethane emulsion is 320000-600000 g / mol.

5. The method for preparing a low-resistance conductive paste according to claim 1, characterized in that: The nano-scale conductive material accounts for 0.01-0.1% of the total weight of the conductive paste.

6. The method for preparing a low-resistance conductive paste according to claim 1, characterized in that: Calculated by weight, the conductive paste includes 5-8 parts of carbon-based conductive material, 10-18 parts of waterborne polyurethane emulsion, and 74-82 parts of ethanol aqueous solution; The solid content of waterborne polyurethane emulsion is 45-55%.

7. The method for preparing a low-resistance conductive paste according to claim 1, characterized in that: The nanoscale conductive material is one or more of carbon nanotubes, multi-walled carbon nanotubes, graphene, and graphene oxide; The carbon-based conductive material is one or more of amorphous carbon, graphene, conductive graphite, carbon nanotubes, and SP.

8. The method for preparing a low-resistance conductive paste according to claim 1, characterized in that: The chain extender is 2,2-bis(hydroxymethyl)propionic acid.

9. A method for preparing a low-resistance carbon-coated aluminum foil, characterized in that: The following steps are involved: A conductive paste is prepared by the method for preparing a low-resistance conductive paste according to any one of claims 1 to 8; The conductive slurry is coated on the aluminum foil and dried to obtain the low-resistance carbon-coated aluminum foil.

10. A low-resistance carbon-coated aluminum foil, characterized in that: The low-resistance carbon-coated aluminum foil is prepared by the method for preparing the low-resistance carbon-coated aluminum foil according to any one of claim 9.