Preparation method of amorphous magnetic powder core

The combination method of preparing spherical amorphous powders through multi-stage atomization method and hydrothermal method for preparation of Fe3O4 nanoparticles, combined with silicone resin coating and rotary pressing technology, solves the problems of complex and high-frequency loss in the preparation process of amorphous alloy powders. , achieving low-pressure and high-density molding and performance improvement.

CN119028689AInactive Publication Date: 2024-11-26TDG HLDG CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411517276.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing amorphous alloy powder preparation methods are complex in technology and irregular in appearance, resulting in poor inductance performance and high high frequency loss, making it difficult to achieve low voltage and high density molding.

Method used

Spherical FeSiBCCr amorphous powder was prepared by multi-stage atomization method, and high-purity Fe3O4 nanoparticles were prepared by hydrothermal method for passivation treatment. Combined with insulating coating of silicone resin, rotary pressing and static magnetic field were applied to achieve low-pressure and high-density molding. .

Benefits of technology

It improves the uniformity and fluidity of the powder coating layer, reduces internal stress, and realizes high-density molding, reduces the loss of amorphous magnetic powder core, improves magnetic permeability, and optimizes DC bias performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028689A_ABST
    Figure CN119028689A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of magnetic materials, in particular to a preparation method of an amorphous magnetic powder core, which comprises the following steps: (1) preparing Fe3O4 nanoparticles; (2) the FeSiBCCr amorphous powder is placed in turbid liquid of Fe3O4 nanometer particles and ethyl alcohol to be subjected to passivating treatment, and passivated FeSiBCCr amorphous powder is obtained; (3) the passivated FeSiBCCr amorphous powder is placed in a mixed solution of organic silicon resin and an organic solvent to be subjected to insulation coating treatment, and finished product powder is obtained after full stirring and drying; and (4) adding a lubricant into the finished product powder, uniformly mixing, putting into a mold, rotating around the longitudinal axis of the mold, applying a magnetic field in the rotating process, pressing, and annealing to obtain the amorphous magnetic powder core with the lowest loss of 125.99 kW / m < 3 > and the highest magnetic conductivity of 46.96 under the test conditions of 100mT and 50kHz, and with the direct current bias of more than 90% under the condition of 100Oe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnetic materials, and in particular to a method for preparing an amorphous magnetic powder core. Background Art

[0002] With the rapid development of the Internet of Things, communication technology, and new energy vehicles, electronic components represented by one-piece molded inductors are constantly developing in the direction of miniaturization, high frequency, and energy saving. As an important component of electronic components, soft magnetic materials are also put forward higher requirements. Compared with traditional crystalline soft magnetic materials, amorphous alloys are considered to be ideal materials for preparing high-performance one-piece molded inductors due to their higher saturation magnetic induction intensity, high resistivity, and low coercivity.

[0003] At present, the main methods for preparing amorphous alloy powders are mechanical ball milling, mechanical crushing and atomization. The patent with publication number CN118039281A discloses a method for preparing an iron-based amorphous magnetic powder core, which requires phosphoric acid coating treatment. The process is relatively complicated. In addition, the amorphous powder is obtained by crushing amorphous strips. The powder morphology is mostly irregular thin blocks with sharp corners. The coating layer is easily damaged during pressing, which is not conducive to the preparation of inductors. The final material loss at 50kHz and 0.1T reaches 320mW / cm 3 The patent with publication number CN118116682A discloses a high permeability and low loss composite magnetic powder core and its preparation method, but its focus is to solve the pressing and molding problem of flaky amorphous powder, and to improve the pressing density by controlling the angle between the iron-based flaky amorphous powder and the pressing direction of the magnetic powder core, while spherical amorphous powder does not have the problem of angle control, and the invention does not involve Fe3O4 coating and particle ratio design.

[0004] Insulation coating is an effective means to reduce the high-frequency loss of amorphous magnetic powder cores. According to whether it has magnetism, the insulating coating materials are mainly divided into two types: non-magnetic materials and magnetic materials. The non-magnetic insulating coating agents are mainly divided into hydrochloric acid and organic resins. The introduction of non-magnetic insulating coating agents can reduce losses, but will sacrifice magnetic permeability. At present, magnetic materials with higher magnetic permeability and resistivity have become ideal insulating coating materials for amorphous alloy powders. The patent with publication number CN117650006A discloses a method for preparing an organic-inorganic insulating coated iron-based composite soft magnetic powder core, in which the inorganic coating material Fe3O4 has high magnetic permeability and high resistivity, but the preparation process is relatively complicated and is not suitable for large-scale production in the industrial field. In addition, the hardness of amorphous alloy powder is high, and the internal stress generated by high pressure during the molding of the magnetic powder core will lead to increased losses. Therefore, how to achieve low-pressure and high-density molding is a key technical issue in the preparation of high-performance one-piece molded inductor devices. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a method for preparing an amorphous magnetic powder core. The following technical scheme is adopted: The present invention discloses a method for preparing an amorphous magnetic powder core, comprising the following steps: Step (1): preparing Fe3O4 nanoparticles, wherein the particle size of the Fe3O4 nanoparticles is 55-150 nm; Step (2): placing FeSiBCCr amorphous powder with a particle size of 10-15 μm in a suspension of Fe3O4 nanoparticles and ethanol for passivation treatment, and obtaining passivated FeSiBCCr amorphous powder after the treatment; Among them, the FeSiBCCr amorphous powder is a spherical amorphous powder prepared by a multi-stage atomization method; Among them, the total mass of FeSiBCCr amorphous powder and Fe3O4 nanoparticles is used as the calculation basis, the mass of FeSiBCCr amorphous powder accounts for 95-99wt%, the mass of Fe3O4 nanoparticles accounts for 1-5wt%, and the mass of ethanol accounts for 5-10wt%; Step (3): placing the passivated FeSiBCCr amorphous powder in a mixed solution of silicone resin and organic solvent for insulation coating treatment, fully stirring and drying to obtain a finished powder; Step (4): Add lubricant to the finished powder, mix well and put into a mold, seal the mold and rotate it around its longitudinal axis, apply a static magnetic field of 0.5-3.5T perpendicular to the longitudinal axis during the rotation, and then press. The pressing pressure is 350-600MPa. After annealing, an iron-based amorphous magnetic powder core is obtained.

[0006] Wherein, in step (1), FeCl3·6H2O is dissolved in a mixed solution of ethylene glycol and diethylene glycol, and after the solute is completely dissolved, sodium acetate and polyethylene glycol are added to the reaction solution in sequence, and after stirring, the reaction solution is transferred into a reaction kettle and placed in a box furnace for heating; after cooling, the product is separated by a magnet, and washed with ethanol and distilled water in sequence; finally, the remaining magnetic particles are placed in a vacuum drying oven for drying, and the desired Fe3O4 nanoparticles can be obtained; Preferably, the mass volume ratio of FeCl3·6H2O, ethylene glycol and diethylene glycol is 1-4g:10-40ml:0-30ml, the mass ratio of FeCl3·6H2O, sodium acetate and polyethylene glycol is 1-4:1-5:1-3, and the hydrothermal treatment conditions are heating at 150-250°C for 5-10h.

[0007] Preferably, the mass volume ratio of FeCl3·6H2O, ethylene glycol and diethylene glycol is 2-3g:20-30ml:10-20ml, the mass ratio of FeCl3·6H2O, sodium acetate and polyethylene glycol is 2-3:2-4:1.5-2, and the hydrothermal treatment condition is heating at 180-200°C for 6-9h.

[0008] Preferably, the FeSiBCCr amorphous powder has a composition of Fe 73 Si 10 B 10 C5Cr2.

[0009] Preferably, the particle size of the Fe3O4 nanoparticles is 60-140nm, preferably 70nm, 80nm, 90nm, 100nm, 110nm, 120nm or 130nm, and the particle size of the FeSiBCCr amorphous powder is 10-15µm, preferably 11µm, 12µm, 13µm or 14µm.

[0010] Preferably, in step (2), the FeSiBCCr amorphous powder is placed in a suspension of Fe3O4 nanoparticles and ethanol for passivation treatment. Based on the total mass of the FeSiBCCr amorphous powder and the Fe3O4 nanoparticles, the mass proportion of the FeSiBCCr amorphous powder is 96-98wt%, preferably 96.5wt%, 97wt% or 97.5wt%, the mass proportion of the Fe3O4 nanoparticles is 2-4wt%, preferably 2.5wt%, 3wt% or 3.5wt%, and the mass proportion of ethanol is 6-9wt%, preferably 6.5wt%, 7wt%, 7.5wt%, 8wt% or 8.5wt%.

[0011] Preferably, in step (3), the total mass of the passivated FeSiBCCr amorphous powder is used as the calculation basis, the mass proportion of the silicone resin in step (3) is 2-5wt%, and the organic solvent is ethanol, and the mass proportion of the ethanol used is 5-10wt%; Preferably, in step (3), the total mass of the passivated FeSiBCCr amorphous powder is used as the calculation basis, the mass proportion of the silicone resin in step (3) is 2.5-4.5wt%, the organic solvent is ethanol, and the mass proportion of the ethanol used is 6-9wt%.

[0012] Preferably, in step (4), the lubricant is barium stearate, and the amount of the lubricant is 0.3-0.5wt% of the mass of the mixed powder; Preferably, in step (4), the lubricant is barium stearate, and the amount of the lubricant is 0.35-0.45 wt % of the mass of the mixed powder.

[0013] Preferably, in step (4), the mold rotation speed is 20-60 r / min, the rotation time is 1-5 h, and a static magnetic field of 0.7-3.2 T is applied perpendicular to the longitudinal axis during the rotation process, and finally pressing is performed at a pressing pressure of 380-580 MPa; Preferably, in step (4), the mold rotation speed is 35-55 r / min, the rotation time is 1.5-4 h, the applied magnetic field strength is 1-3 T, and the pressing pressure is 400-550 MPa; Preferably, in step (4), the mold rotation speed is 40 r / min, 45 r / min or 50 r / min, the rotation time is 2 h, 2.5 h, 3 h or 3.5 h, the applied magnetic field strength is 1.5 T, 2 T or 2.5 T, and the pressing pressure is 420 MPa, 450 MPa, 480 MPa, 500 MPa or 520 MPa.

[0014] Preferably, in step (4), the stress relief annealing temperature is 350-450° C., the holding time is 60-150 min, and the heating rate is 7-12° C. / min.

[0015] The present invention has the following beneficial effects: The present invention adopts a multi-stage atomization method to prepare spherical amorphous powder, and the coating layer during coating is more uniform, and the coating layer will not be damaged during pressing; the method of preparing Fe3O4 nanoparticles by a hydrothermal method has a simple preparation process, is non-toxic, and is suitable for industrial-scale production; wherein the Fe3O4 nanoparticles have high purity and crystallinity, and have a high saturation magnetization intensity (above 92emu / g), which is beneficial to improving the magnetic permeability and DC bias performance; before pressing, the mold containing the finished powder is rotated, and a static magnetic field is applied at the same time, which can improve the fluidity and uniformity of the powder, and the gaps between the powders can be filled with each other, thereby reducing the internal stress of the material pressing and realizing high-density low-pressure molding. Furthermore, the loss of the obtained amorphous magnetic powder core under the test conditions of 100mT and 50kHz can reach a minimum of 125.99kW / m 3 The magnetic permeability can reach up to 46.96, and the DC bias under 100Oe conditions exceeds 90%. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the scanning electron microscope image of FeSiBCCr amorphous powder; Figure 2 is a graph showing the relationship between the magnetic permeability and the frequency of the embodiment and the comparative example; Figure 3 This is a graph showing the relationship between the loss and frequency of the embodiment and the comparative example under the 100mT test condition. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the amorphous coating material, amorphous powder core material and preparation method thereof provided by the present invention are further described in detail below through embodiments and in combination with the accompanying drawings.

[0018] Example 1 is as follows: A method for preparing an amorphous magnetic powder core of the present invention comprises the following specific steps: Step (1): 1.35 g of FeCl3·6H2O is weighed and dissolved in a mixed solution of 10 ml of ethylene glycol and 20 ml of diethylene glycol. After the solute is completely dissolved, 3.6 g of sodium acetate and 1.0 g of polyethylene glycol are added to the reaction solution in sequence. After magnetic stirring at 60° C. for 30 min, the reaction solution is transferred into a high-pressure reactor and placed in a box furnace for heat treatment at 200° C. for 8 h. After cooling, the product is separated by a magnet and washed with ethanol and distilled water in sequence. Finally, the remaining magnetic particles are placed in a vacuum drying oven at 60° C. and dried for 6 h to obtain the desired Fe3O4 nanoparticles. Step (2): Spherical FeSiBCCr amorphous powder is prepared by multi-stage atomization method, the morphology is shown in Figure 1 , 99.0 g of FeSiBCCr amorphous powder was weighed and placed in a suspension of 1.0 g of Fe3O4 nanoparticles and 6 g of ethanol for passivation treatment to obtain passivated FeSiBCCr amorphous powder; Step (3): Weigh 100 g of passivated FeSiBCCr amorphous powder and place it in a mixed solution of silicone resin and ethanol for insulation coating treatment, wherein the silicone resin used for the insulation coating treatment accounts for 4 wt % of the passivated amorphous powder, and the ethanol accounts for 10 wt % of the passivated amorphous powder, and the finished powder is obtained after sufficient stirring and drying; Step (4): adding 0.3 wt % of barium stearate to the finished powder, placing the mixture in a mold, and rotating the mixture around the longitudinal axis at a speed of 25 r / min for 4 h, while applying a 1.5 T magnetic field perpendicular to the longitudinal axis, and then preparing a ring-shaped material with an outer diameter of 14 mm and an inner diameter of 8 mm under a pressure of 400 MPa; Step (5): The above material is subjected to stress relief annealing treatment at 400° C. for 100 min to obtain an amorphous powder core.

[0019] Example 2 is as follows: A method for preparing an amorphous magnetic powder core of the present invention comprises the following specific steps: Step (1): 1.35 g of FeCl3·6H2O is weighed and dissolved in a mixed solution of 10 ml of ethylene glycol and 20 ml of diethylene glycol. After the solute is completely dissolved, 3.6 g of sodium acetate and 1.0 g of polyethylene glycol are added to the reaction solution in sequence. After magnetic stirring at 60° C. for 30 min, the reaction solution is transferred into a high-pressure reactor and placed in a box furnace for heat treatment at 200° C. for 8 h. After cooling, the product is separated by a magnet and washed with ethanol and distilled water in sequence. Finally, the remaining magnetic particles are placed in a vacuum drying oven at 60° C. and dried for 6 h to obtain the desired Fe3O4 nanoparticles. Step (2): 98.0 g of spherical FeSiBCCr amorphous powder prepared by a multi-stage atomization method was weighed and placed in a suspension of 2.0 g of Fe3O4 nanoparticles and 8 g of ethanol for passivation treatment to obtain passivated FeSiBCCr amorphous powder; Step (3): Weigh 100 g of passivated FeSiBCCr amorphous powder and place it in a mixed solution of silicone resin and ethanol for insulation coating treatment, wherein the silicone resin used for the insulation coating treatment accounts for 3 wt % of the passivated amorphous powder, and the ethanol accounts for 8 wt % of the passivated amorphous powder. After fully stirring and drying, a finished powder is obtained; Step (4): adding 0.4 wt % of barium stearate to the finished powder, placing the mixture in a mold, and rotating the mixture around the longitudinal axis at a speed of 30 r / min for 3 h, while applying a 2 T magnetic field perpendicular to the longitudinal axis, and then preparing a ring-shaped material with an outer diameter of 14 mm and an inner diameter of 8 mm under a pressure of 580 MPa; Step (5): The above material is subjected to stress relief annealing treatment at 450° C. for 120 min to obtain an amorphous powder core.

[0020] Example 3 is as follows: A method for preparing an amorphous magnetic powder core of the present invention comprises the following specific steps: Step (1): 1.35 g of FeCl3·6H2O is weighed and dissolved in a mixed solution of 10 ml of ethylene glycol and 20 ml of diethylene glycol. After the solute is completely dissolved, 3.6 g of sodium acetate and 1.0 g of polyethylene glycol are added to the reaction solution in sequence. After magnetic stirring at 60° C. for 30 min, the reaction solution is transferred into a high-pressure reactor and placed in a box furnace for heat treatment at 200° C. for 8 h. After cooling, the product is separated by a magnet and washed with ethanol and distilled water in sequence. Finally, the remaining magnetic particles are placed in a vacuum drying oven at 60° C. and dried for 6 h to obtain the desired Fe3O4 nanoparticles. Step (2): 97.0 g of spherical FeSiBCCr amorphous powder prepared by a multi-stage atomization method was weighed and placed in a suspension of 3.0 g of Fe3O4 nanoparticles and 8 g of ethanol for passivation treatment to obtain a passivated FeSiBCCr amorphous powder; Step (3): Weigh 100 g of passivated FeSiBCCr amorphous powder and place it in a mixed solution of silicone resin and ethanol for insulation coating treatment, wherein the silicone resin used for the insulation coating treatment accounts for 2 wt % of the passivated amorphous powder, and the ethanol accounts for 8 wt % of the passivated amorphous powder. After fully stirring and drying, a finished powder is obtained; Step (4): adding 0.5 wt % of barium stearate to the finished powder, placing the mold, and rotating the mold around the longitudinal axis at a speed of 40 r / min for 3.5 h, while applying a 1 T magnetic field perpendicular to the longitudinal axis, and then preparing a ring-shaped material with an outer diameter of 14 mm and an inner diameter of 8 mm under a pressure of 500 MPa; Step (5): The above material is subjected to stress relief annealing treatment at 400° C. for 150 min to obtain an amorphous powder core.

[0021] Embodiment 4 is as follows: A method for preparing an amorphous magnetic powder core of the present invention comprises the following specific steps: Step (1): 1.35 g of FeCl3·6H2O is weighed and dissolved in a mixed solution of 10 ml of ethylene glycol and 20 ml of diethylene glycol. After the solute is completely dissolved, 3.6 g of sodium acetate and 1.0 g of polyethylene glycol are added to the reaction solution in sequence. After magnetic stirring at 60° C. for 30 min, the reaction solution is transferred into a high-pressure reactor and placed in a box furnace for heat treatment at 200° C. for 8 h. After cooling, the product is separated by a magnet and washed with ethanol and distilled water in sequence. Finally, the remaining magnetic particles are placed in a vacuum drying oven at 60° C. and dried for 6 h to obtain the desired Fe3O4 nanoparticles. Step (2): 96.0 g of spherical FeSiBCCr amorphous powder prepared by a multi-stage atomization method was weighed and placed in a suspension of 4.0 g of Fe3O4 nanoparticles and 9 g of ethanol for passivation treatment to obtain passivated FeSiBCCr amorphous powder; Step (3): Weigh 100 g of passivated FeSiBCCr amorphous powder and place it in a mixed solution of silicone resin and ethanol for insulation coating treatment, wherein the silicone resin used for the insulation coating treatment accounts for 5 wt % of the passivated amorphous powder, and the ethanol accounts for 10 wt % of the passivated amorphous powder, and the finished powder is obtained after sufficient stirring and drying; Step (4): adding 0.35 wt % of barium stearate to the finished powder, placing the mixture in a mold, and rotating the mixture around the longitudinal axis at a speed of 50 r / min for 4.5 h, while applying a 2.5 T magnetic field perpendicular to the longitudinal axis, and then preparing a ring-shaped material with an outer diameter of 14 mm and an inner diameter of 8 mm under a pressure of 420 MPa; Step (5): The above material is subjected to stress relief annealing treatment at 350° C. for 60 minutes to obtain an amorphous powder core.

[0022] Comparative Example 1 is as follows: The only difference between Comparative Example 1 and Example 4 is that the FeSiBCCr amorphous powder is not coated with Fe3O4 nanoparticles.

[0023] Comparative Example 2 is as follows: The only difference between Comparative Example 2 and Example 3 is that after adding 0.6 wt % of barium stearate to the finished powder, the finished powder is directly pressed at a pressure of 500 MPa at room temperature without being treated with a magnetic field.

[0024] The present invention uses a scanning electron microscope to observe the morphology of FeSiBCCr amorphous powder. The results are as follows: Figure 1 As shown, the FeSiBCCr amorphous powder prepared by the multi-stage atomization method is regular spherical.

[0025] After testing, from Figure 2 It can be seen that the effective magnetic permeability of the magnetic powder core obtained in the embodiment under the test conditions of 1V and 100kHz is significantly higher than that of the comparative example, and the maximum value can reach 46.96. Figure 3 It can be seen that the loss under the test conditions of 100mT and 50kHz is significantly lower than that of the control group, and the minimum can reach 125.99kW / m 3 ,From Table 1, it can be seen that the DC superposition ,performance under the 100Oe test condition is significantly higher than the control ,example, and can reach 92.08% at the highest.

[0026] Table 1 shows the DC superposition performance results of the embodiments and comparative examples.

[0027] The embodiments described above provide a detailed description of the technical solutions of the present invention. It should be understood that the above descriptions are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, supplements or equivalent substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an amorphous magnetic powder core, characterized in that: The steps include: Step (1): preparing Fe3O4 nanoparticles, wherein the particle size of the Fe3O4 nanoparticles is 55-150 nm; Step (2): placing FeSiBCCr amorphous powder with a particle size of 10-15 μm in a suspension of Fe3O4 nanoparticles and ethanol for passivation treatment, and obtaining passivated FeSiBCCr amorphous powder after the treatment; Among them, the FeSiBCCr amorphous powder is a spherical amorphous powder prepared by a multi-stage atomization method; Among them, the total mass of FeSiBCCr amorphous powder and Fe3O4 nanoparticles is used as the calculation basis, the mass of FeSiBCCr amorphous powder accounts for 95-99wt%, the mass of Fe3O4 nanoparticles accounts for 1-5wt%, and the mass of ethanol accounts for 5-10wt%; Step (3): placing the passivated FeSiBCCr amorphous powder in a mixed solution of silicone resin and organic solvent for insulation coating treatment, fully stirring and drying to obtain a finished powder; Step (4): Add lubricant to the finished powder, mix well and put into a mold, seal the mold and rotate it around its longitudinal axis, apply a static magnetic field of 0.5-3.5T perpendicular to the longitudinal axis during the rotation, and then press. The pressing pressure is 350-600MPa. After annealing, an iron-based amorphous magnetic powder core is obtained.

2. The method for preparing an amorphous magnetic powder core according to claim 1, characterized in that: In the step (1), FeCl3·6H2O is dissolved in a mixed solution of ethylene glycol and diethylene glycol, and after the solute is completely dissolved, sodium acetate and polyethylene glycol are added to the reaction solution in sequence, and after stirring, the reaction solution is transferred into a reaction kettle and placed in a box furnace for heating, and after cooling, the product is separated by a magnet, and washed with ethanol and distilled water in sequence; finally, the remaining magnetic particles are placed in a vacuum drying oven for drying, and the desired Fe3O4 nanoparticles can be obtained.

3. The method for preparing an amorphous magnetic powder core according to claim 2, characterized in that: The mass volume ratio of FeCl3·6H2O, ethylene glycol and diethylene glycol is 1-4g:10-40ml:0-30ml, the mass ratio of FeCl3·6H2O, sodium acetate and polyethylene glycol is 1-4:1-5:1-3, and the hydrothermal treatment condition is heating at 150-250°C for 5-10h.

4. The method for preparing an amorphous magnetic powder core according to claim 1, characterized in that: The FeSiBCCr amorphous powder is composed of Fe 73 Si 10 B 10 C5Cr2.

5. The method for preparing an amorphous magnetic powder core according to claim 1, characterized in that: The particle size of the Fe3O4 nanoparticles is 60-140nm, and the particle size of the FeSiBCCr amorphous powder is 10-15µm.

6. The method for preparing an amorphous magnetic powder core according to claim 1, characterized in that: In the step (2), the FeSiBCCr amorphous powder is placed in a suspension of Fe3O4 nanoparticles and ethanol for passivation treatment. The total mass of the FeSiBCCr amorphous powder and the Fe3O4 nanoparticles is used as the calculation basis, and the mass proportion of the FeSiBCCr amorphous powder is 96-98wt%, the mass proportion of the Fe3O4 nanoparticles is 2-4wt%, and the mass proportion of the ethanol is 6-9wt%.

7. The method for preparing an amorphous magnetic powder core according to claim 1, characterized in that: In the step (3), the total mass of the passivated FeSiBCCr amorphous powder is used as the calculation basis, the mass proportion of the silicone resin in the step (3) is 2-5wt%, and the organic solvent is ethanol, and the mass proportion of the ethanol used is 5-10wt%.

8. The method for preparing an amorphous magnetic powder core according to claim 1, characterized in that: In the step (4), the lubricant is barium stearate, and the amount of the lubricant is 0.3-0.5wt% of the mass of the mixed powder.

9. The method for preparing an amorphous magnetic powder core according to claim 1, characterized in that: In the step (4), the mold rotation speed is 20-60 r / min, the rotation time is 1-5 h, the magnetic field applied during the rotation is 0.7-3.2 T, and the pressing pressure is 380-580 MPa.

10. The method for preparing an amorphous magnetic powder core according to claim 1, characterized in that: In the step (4), the stress relief annealing temperature is 350-450° C., the holding time is 60-150 min, and the heating rate is 7-12° C. / min.

Citation Information

Patent Citations

  • Organic-inorganic insulation coated iron-based composite soft magnetic powder core and preparation method thereof

    CN117650006A

  • Iron-based amorphous magnetic powder core and preparation method thereof

    CN118039281A

  • Composite magnetic powder core with high magnetic conductivity and low loss and preparation method thereof

    CN118116682A

  • Preparation method of circle-oriented non-crystal magnetic powder core

    CN105097167A

  • Ferroferric oxide nano-microsphere with adjustable grain size and magnetic response and preparation method of ferroferric oxide nano-microsphere

    CN116332240A