Copper interconnection dielectric layer structure preparation method and copper interconnection dielectric layer structure
By directly depositing amorphous boron nitride film and other materials in the copper interconnect dielectric layer structure, the problems of high dielectric constant and weak mechanical properties of the ULK film are solved, and the effect of reducing parasitic capacitance and simplifying the process is achieved.
Patent Information
- Application Number
- CN202310581865.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
The ULK film layer in the existing copper interconnect dielectric layer structure has a high dielectric constant and weak mechanical properties, resulting in large parasitic capacitance and complex preparation process, which increases production costs.
Direct deposition of amorphous boron nitride film layer is used as the ultra-low dielectric constant dielectric layer, combining silicon nitride layer, silicon carbon oxide layer and metal mask layer, the deposition process of the TEOS layer is omitted, and adhesion and mechanical properties are improved.
The inter-line capacitance is reduced, the mechanical properties and adhesion of the dielectric layer are improved, the process steps are simplified, and the production costs are reduced.
Smart Images

Figure CN119028904A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of integrated circuit manufacturing, and in particular to a method for preparing a copper interconnect dielectric layer structure and a copper interconnect dielectric layer structure. Background Art
[0002] The parasitic capacitance of transistor interconnect structures is the main factor affecting transistor performance. As transistor size continues to decrease, in order to reduce parasitic capacitance, the design of copper interconnect dielectric layers based on low dielectric constant films has become a current research hotspot.
[0003] In terms of the film properties and preparation process of the ultra-low dielectric constant (ULK) layer of the copper interconnect dielectric layer structure, the preparation process of the annular structure ULK film layer in the existing interconnect structure is to first deposit a thin film and then treat it with ultraviolet light to form a porous structure. The dielectric constant k of the prepared ULK film layer is 2.47 and the hardness is 1.1Gpa. Although the dielectric constant can be reduced by introducing air with a lower dielectric constant, the porous structure also causes the mechanical properties of the ULK film layer to be very weak. In addition, in the copper interconnect dielectric layer structure design, the metal layer is used to set the copper wire. In the existing metal layer, after the silicon carbonitride (NDC) layer is deposited on the substrate, it is necessary to first grow a silicon dioxide layer (commonly referred to as a TEOS layer) with tetraethyl orthosilicate (TEOS) as a precursor on the NDC layer, and then deposit the ULK layer. Since the prepared ULK layer has poor adhesion, the process of depositing the TEOS layer is added to provide adhesion and mechanical support for the ULK layer, which increases the cost of device generation. Therefore, how to reduce the capacitance between wires while improving mechanical properties and saving process costs is a technical problem that technical personnel in this field currently need to solve. Summary of the invention
[0004] The purpose of the present application is to provide a method for preparing a copper interconnect dielectric layer structure and a copper interconnect dielectric layer structure, thereby reducing the capacitance between lines while improving mechanical properties and saving process costs.
[0005] To achieve the above-mentioned purpose, the present application provides a method for preparing a copper interconnect dielectric layer structure, comprising:
[0006] Depositing a protective layer on the surface of the substrate to protect the copper in the pre-deposited copper interconnect dielectric layer structure;
[0007] An amorphous boron nitride film layer is deposited on the surface of the protective layer as an ultra-low dielectric constant dielectric layer to form the copper interconnect dielectric layer structure.
[0008] Optionally, after depositing an amorphous boron nitride film layer on the surface of the protective layer as the ultra-low dielectric constant dielectric layer, the method further comprises:
[0009] A silicon carbonitride layer, a silicon carbide layer, a metal mask layer and a silicon dioxide layer are sequentially deposited on the surface of the amorphous boron nitride film layer.
[0010] Optionally, the protective layer is a silicon carbonitride layer.
[0011] Optionally, depositing a protective layer on the surface of the substrate includes:
[0012] Tetramethylsilane and ammonia are used as precursors and an inert gas is used as a carrier gas to deposit the silicon carbonitride layer on the surface of the substrate.
[0013] Optionally, the step of depositing the silicon carbonitride layer on the surface of the substrate using tetramethylsilane and ammonia as precursors and an inert gas as a carrier gas comprises:
[0014] The silicon carbonitride layer is deposited on the surface of the substrate by using plasma enhanced chemical vapor deposition equipment, tetramethylsilane and ammonia as precursors and inert gas as carrier gas.
[0015] Optionally, depositing an amorphous boron nitride film layer on the surface of the protective layer as an ultra-low dielectric constant dielectric layer includes:
[0016] The amorphous boron nitride film layer is deposited on the surface of the protective layer as the ultra-low dielectric constant dielectric layer using boron nitride as a precursor in a hydrogen flow at a preset temperature.
[0017] Optionally, depositing the amorphous boron nitride film layer as the ultra-low dielectric constant dielectric layer on the surface of the protective layer using boron nitride as a precursor in a hydrogen flow at the preset temperature includes:
[0018] The amorphous boron nitride film layer is deposited as the ultra-low dielectric constant dielectric layer on the surface of the protective layer using inductively coupled plasma chemical vapor deposition equipment at a preset temperature in a hydrogen flow using boron nitride as a precursor.
[0019] Optionally, the preset temperature is 350° C. to 400° C., including values at both ends.
[0020] Optionally, the thickness of the amorphous boron nitride film layer is greater than or equal to
[0021] To achieve the above-mentioned purpose, the present application also provides a copper interconnect dielectric layer structure, including: a copper interconnect dielectric layer structure prepared by the copper interconnect dielectric layer structure preparation method described above.
[0022] The present application provides a method for preparing a copper interconnect dielectric layer structure, which directly deposits an amorphous boron nitride film layer as an ultra-low dielectric constant layer. Compared with the ultra-low dielectric constant film layer of a ring structure in an existing interconnect structure with a dielectric constant k of 2.47 and a hardness of 1.1 GPa, since the dielectric constant k of amorphous boron nitride is less than 1.78 and the hardness is greater than 11 GPa, while ensuring that the ultra-low dielectric constant dielectric layer has a lower dielectric constant, the hardness of the ultra-low dielectric constant dielectric layer in the metal layer can be improved, thereby improving the mechanical properties of the ultra-low dielectric constant dielectric layer; since the ultra-low dielectric constant dielectric layer is formed by directly depositing amorphous boron nitride, the optical processing process in the preparation process of the metal layer can be omitted, thereby improving the production capacity of the device; since the amorphous boron nitride has strong adhesion, the adhesion of the ultra-low dielectric constant dielectric layer in the metal layer can be enhanced, so the process of depositing a TEOS layer in the preparation process of the metal layer can be omitted, thereby simplifying the process steps in the product process and reducing the production cost of the device. The present application also provides a copper interconnect dielectric layer structure. The ultra-low dielectric constant dielectric layer in the present application has stronger mechanical properties and stronger adhesion than the annular structure ultra-low dielectric constant film layer in the existing interconnect structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.
[0024] Figure 1 A flow chart of the process for preparing the ring-shaped ultra-low dielectric constant thin film in the existing copper interconnect dielectric layer design;
[0025] Figure 2 A flow chart of a method for preparing a copper interconnect dielectric layer structure provided in an embodiment of the present application;
[0026] Figure 3 A flow chart of another method for preparing a copper interconnect dielectric layer structure provided in an embodiment of the present application;
[0027] Figure 4 A dielectric layer structure diagram of a metal layer M1 provided in an embodiment of the present application;
[0028] Figure 5 A dielectric layer structure diagram of a metal layer M6 provided in an embodiment of the present application.
[0029] Attached Figure 4 and 5 In the figure, the reference numerals are described as follows:
[0030] 01-N well; 02-P well; 1-silicon carbon nitride layer; 2-amorphous boron nitride film layer; 3-silicon carbide layer; 4-metal mask layer; 5-silicon dioxide layer. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0032] As transistor size decreases and circuit density increases, resistance and capacitance delays affect signal transmission speed. Parasitic capacitance is proportional to the relative dielectric constant of the insulating film and the cross-sectional area of the wiring, and inversely proportional to the wiring spacing. The process limits the use of geometric changes to reduce parasitic capacitance, so low dielectric constant materials are widely used. With the miniaturization of the process, the wiring cross-sectional area and wiring spacing are getting smaller and smaller, and the capacitance between wiring increases accordingly. Therefore, the copper interconnect dielectric layer design based on low dielectric constant film has become an inevitable choice for the development of integrated circuit technology.
[0033] Please refer to the attached Figure 1 In the existing HK Flow (high dielectric constant insulating layer process), the back-end ULK layer uses methyl diethoxysilane (DEMS) and porogen α-terpinene (ATRP) as precursors, and the reaction forms an internal ring-shaped structure film, and the impurity bond is eliminated by ultraviolet light treatment to form a porous structure, and the air with a lower dielectric constant is introduced to reduce the dielectric constant. However, there is a defect of weak mechanical properties in the porous structure ultra-low dielectric constant film. In addition, due to the poor adhesion of the ULK layer, it is necessary to grow a TEOS layer on the NDC layer before depositing the ULK layer in the metal layer, and provide mechanical support and adhesion for the ULK layer through the dense film and silicon-oxygen bond of the TEOS layer, so it also causes the increase of the device production cost.
[0034] Although the existing technical solutions can reduce the dielectric constant of the film and reduce the capacitance between wires, the wiring cross-sectional area and wiring spacing of the advanced process are further reduced, and the porous structure ultra-low dielectric constant film has the defect of weak mechanical properties and high device production cost. Therefore, the present application provides a method for preparing a copper interconnect dielectric layer structure, by directly depositing an amorphous boron nitride film layer as an ultra-low dielectric constant dielectric layer, thereby reducing the capacitance between wires while improving the mechanical properties and saving process costs.
[0035] Please refer to Figure 2 , Figure 2A flow chart of a method for preparing a copper interconnect dielectric layer structure provided in an embodiment of the present application, the method may include:
[0036] S101: depositing a protective layer on the surface of the substrate to protect the copper in the pre-deposited copper interconnect dielectric layer structure.
[0037] It should be noted that when manufacturing a semiconductor integrated circuit, multiple metal layers (metal interconnects are provided in the metal layers, and copper is generally selected as the metal interconnect material) can be provided on the surface of the substrate according to different needs to achieve electrical interconnection between the layers. In order to protect the copper in the pre-deposited copper interconnect dielectric layer structure, a protective layer needs to be deposited on the surface of the substrate. This embodiment does not limit the specific type of the protective layer, as long as it can protect the copper in the pre-deposited copper interconnect dielectric layer structure, for example, the protective layer can be a silicon carbonitride layer.
[0038] This embodiment does not limit the specific method of depositing the protective layer. The corresponding deposition method can be determined according to the specific type of the protective layer. For example, when the protective layer is a silicon carbonitride layer, tetramethylsilane and ammonia can be used as precursors, and an inert gas can be used as a carrier gas to deposit the silicon carbonitride layer on the substrate surface. This embodiment does not limit the specific flow ratio of tetramethylsilane and ammonia, and the specific flow ratio of tetramethylsilane and ammonia can be determined according to the target thickness of the silicon carbonitride layer. This embodiment does not limit the specific type of inert gas, as long as it can ensure that it does not react with tetramethylsilane and ammonia, for example, helium can be used as a carrier gas. This embodiment does not limit the specific equipment for depositing the silicon carbonitride layer, as long as it is ensured that tetramethylsilane and ammonia as precursors, and an inert gas as a carrier gas are passed into the equipment to deposit the silicon carbonitride layer on the substrate surface, for example, a plasma enhanced chemical vapor deposition equipment can be used. This embodiment does not limit the specific temperature for depositing the silicon carbonitride layer, and the specific temperature for depositing the silicon carbonitride layer can be determined according to actual conditions. For example, the temperature for depositing the silicon carbonitride layer can be 350°C to 400°C, and includes the values at both ends. This embodiment does not limit the specific thickness of the silicon carbonitride layer. The specific thickness of the silicon carbonitride layer can be determined according to actual conditions. For example, the thickness of the silicon carbonitride layer can be The present embodiment does not limit the specific refractive index of the silicon carbonitride layer, and the specific refractive index of the silicon carbonitride layer may be determined according to actual conditions. For example, the refractive index of the silicon carbonitride layer may be 1.86 to 1.96.
[0039] S102: depositing an amorphous boron nitride film layer on the surface of the protective layer as an ultra-low dielectric constant dielectric layer to form a copper interconnect dielectric layer structure.
[0040] It should be noted that amorphous boron nitride is composed of boron and nitrogen atoms and has an amorphous structure. The dielectric constant value of the annular ultra-low dielectric constant film layer in the existing interconnect structure is 2.47. Thanks to the non-polar bonds and disordered structure between boron nitrides, the arrangement of dipoles is prevented, making the dielectric constant value k of amorphous boron nitride less than 1.78. By depositing an amorphous boron nitride film layer as an ultra-low dielectric constant dielectric layer, the dielectric constant of the ultra-low dielectric constant dielectric layer can be reduced, so that the parasitic capacitance can be more significantly reduced, thereby improving signal transmission efficiency. The ultra-low dielectric constant dielectric layer of amorphous boron nitride is used as a diffusion barrier layer in the copper interconnect dielectric layer structure to block copper diffusion.
[0041] This embodiment does not limit the specific method of depositing the amorphous boron nitride film layer, as long as it is ensured that an amorphous boron nitride film layer can be formed on the surface of the protective layer. For example, it can be deposited on the surface of the protective layer as an ultra-low dielectric constant dielectric layer using boron nitride as a precursor in a hydrogen flow at a preset temperature. This embodiment does not limit the specific equipment for depositing the amorphous boron nitride film layer, as long as it is ensured that the boron nitride as a precursor and hydrogen are passed into the equipment to deposit an amorphous boron nitride film layer on the surface of the protective layer. For example, an inductively coupled plasma chemical vapor deposition device can be used. This embodiment does not limit the specific flow rate of boron nitride, and the specific flow rate of boron nitride can be determined according to the target thickness of the amorphous boron nitride film layer. This embodiment does not limit the specific value of the preset temperature, and the specific value of the preset temperature can be determined according to actual conditions. For example, the preset temperature can be 350℃~400℃, and includes the values at both ends. This embodiment does not limit the specific thickness of the amorphous boron nitride film layer, and the specific thickness of the amorphous boron nitride film layer can be determined according to actual conditions. For example, the thickness of the amorphous boron nitride film layer can be greater than or equal to This embodiment does not limit the specific refractive index of the amorphous boron nitride film layer, and the specific refractive index of the amorphous boron nitride film layer can be determined according to actual conditions. For example, the refractive index of the amorphous boron nitride film layer can be 1.31 to 1.43, including both ends.
[0042] It should be noted that the copper interconnect dielectric layer structure prepared in this embodiment is used as a metal interlayer dielectric layer. After the preparation of the copper interconnect dielectric layer structure is completed, grooves for arranging copper wires will be further etched in the prepared copper interconnect dielectric layer structure, and copper will be plated in the grooves to complete the preparation of the metal layer. When depositing each metal layer, the copper interconnect dielectric layer structure preparation method of this embodiment can be used to prepare the copper interconnect dielectric layer structure required for the metal layer.
[0043] Furthermore, after depositing an amorphous boron nitride film layer as an ultra-low dielectric constant dielectric layer on the surface of the protective layer, this embodiment can also sequentially deposit a silicon carbonitride layer, a silicon carbide layer, a metal mask layer and a silicon dioxide layer on the surface of the amorphous boron nitride film layer.
[0044] Based on the above embodiments, the present application directly deposits an amorphous boron nitride film layer as an ultra-low dielectric constant layer. Compared with the annular structure ultra-low dielectric constant film layer in the existing interconnect structure with a dielectric constant k of 2.47 and a hardness of 1.1 GPa, since the dielectric constant k of amorphous boron nitride is less than 1.78 and the hardness is greater than 11 GPa, while ensuring that the ultra-low dielectric constant layer has a lower dielectric constant, the hardness of the ultra-low dielectric constant layer in the metal layer can be improved, thereby improving the mechanical properties of the ultra-low dielectric constant layer; since the ultra-low dielectric constant layer is formed by directly depositing amorphous boron nitride, the light treatment process in the preparation process of the metal layer can be omitted, thereby simplifying the process steps in the product manufacturing process; since amorphous boron nitride has strong adhesion, the adhesion of the ultra-low dielectric constant layer in the metal layer can be enhanced, so the process of depositing the TEOS layer in the preparation process of the metal layer can be omitted, thereby simplifying the process steps in the product manufacturing process and reducing the production cost of the device.
[0045] Please refer to Figure 3 , Figure 3 A flow chart of another method for preparing a copper interconnect dielectric layer structure provided in an embodiment of the present application, the method may include:
[0046] S201: using plasma enhanced chemical vapor deposition equipment, tetramethylsilane and ammonia as precursors, and an inert gas as a carrier gas to deposit a silicon carbonitride layer on the substrate surface to protect the copper in the pre-deposited copper interconnect dielectric layer structure.
[0047] S202: using an inductively coupled plasma chemical vapor deposition device, at a preset temperature, in a hydrogen flow, using boron nitride as a precursor, depositing an amorphous boron nitride film layer as an ultra-low dielectric constant dielectric layer on the surface of the protective layer.
[0048] S203: depositing a silicon carbonitride layer, a silicon carbide layer, a metal mask layer and a silicon dioxide layer in sequence on the surface of the amorphous boron nitride film layer to form a copper interconnect dielectric layer structure.
[0049] It should be noted that the silicon dioxide layer is used as a covering layer to block the photoresist during the etching process; the etching rates between different film layers are different, and the deposited metal mask layer can be used to adjust the etching rate; the silicon oxycarbide layer is used as a buffer layer to block the photoresist during the etching process.
[0050] The present embodiment does not limit the specific thickness of the silicon carbon nitride layer, and the specific thickness of the silicon carbon nitride layer can be determined according to actual conditions. The present embodiment does not limit the specific method of depositing the silicon carbide layer, as long as it is ensured that the silicon carbide layer can be formed on the surface of the silicon nitride layer, for example, a plasma enhanced chemical vapor deposition device can be used to deposit the silicon carbide layer on the surface of the silicon nitride layer. The present embodiment does not limit the specific thickness of the silicon carbide layer, and the specific thickness of the silicon carbide layer can be determined according to actual conditions. The present embodiment does not limit the specific method of depositing the metal mask layer, as long as it is ensured that the metal mask layer can be formed on the surface of the silicon carbide layer, for example, a plasma enhanced chemical vapor deposition device can be used to deposit the metal mask layer on the surface of the silicon carbide layer. The present embodiment does not limit the specific thickness of the metal mask layer, and the specific thickness of the metal mask layer can be determined according to actual conditions. The present embodiment does not limit the specific method of depositing the silicon dioxide layer, as long as it is ensured that the silicon dioxide layer can be formed on the surface of the metal mask layer, for example, a plasma enhanced chemical vapor deposition device can be used to deposit the silicon dioxide layer on the surface of the metal mask layer. The present embodiment does not limit the specific thickness of the silicon dioxide layer, and the specific thickness of the silicon dioxide layer can be determined according to actual conditions.
[0051] It should be noted that when depositing each metal layer, the copper interconnect dielectric layer structure preparation method of this embodiment can be used to prepare the copper interconnect dielectric layer structure required for the metal layer.
[0052] Based on the above embodiments, the present application deposits a silicon carbon nitride layer on the substrate surface of the wafer by plasma enhanced chemical vapor deposition equipment, and deposits an amorphous boron nitride layer on the surface of the silicon carbon nitride layer by inductively coupled plasma chemical vapor deposition equipment to serve as the substrate for the subsequent copper interconnect dielectric layer structure. Compared with the annular structure ultra-low dielectric constant film layer in the existing interconnect structure with a dielectric constant k of 2.47 and a hardness of 1.1 GPa, since the dielectric constant k of amorphous boron nitride is less than 1.78 and the hardness is greater than 11 GPa, while ensuring that the ultra-low dielectric constant dielectric layer has a lower dielectric constant, the hardness of the ultra-low dielectric constant dielectric layer in the metal layer can be improved, thereby improving the mechanical properties of the ultra-low dielectric constant dielectric layer; since the ultra-low dielectric constant dielectric layer is formed by directly depositing amorphous boron nitride, the light treatment process in the preparation process of the metal layer can be omitted, thereby simplifying the process steps in the product process; since amorphous boron nitride has strong adhesion, the adhesion of the ultra-low dielectric constant dielectric layer in the metal layer can be enhanced, so the process of depositing the TEOS layer in the preparation process of the metal layer can be omitted, thereby simplifying the process steps in the product process and reducing the production cost of the device.
[0053] The present application also provides a copper interconnect dielectric layer structure, including: a copper interconnect dielectric layer structure prepared by the copper interconnect dielectric layer structure preparation method described above.
[0054] Based on the above embodiments, the ultra-low dielectric constant dielectric layer manufactured in the present application has stronger mechanical properties and stronger adhesion than the ultra-low dielectric constant film layer with a ring structure in the existing interconnect structure.
[0055] The following is a specific example to illustrate the copper interconnect dielectric layer structure preparation process. Figure 4 and Figure 5 , Figure 4 A dielectric layer structure diagram of a metal layer M1 provided in an embodiment of the present application; Figure 5 A dielectric layer structure diagram of a metal layer M6 provided in an embodiment of the present application.
[0056] Example 1
[0057] In the metal layer M1 (the first metal layer), tetramethylsilane (4MS) and ammonia (NH3) are used as precursors, helium (He) is used as a carrier gas, and a plasma enhanced chemical vapor deposition (PECVD) device is used to deposit the metal layer M1 on the device surface at 400°C. The silicon carbonitride layer 1 is used as a substrate, and boron nitride benzene is used as a precursor. An amorphous boron nitride (a-BN) layer 2 is formed by a one-step reaction at 400°C in a hydrogen flow through an inductively coupled plasma chemical vapor deposition (ICP-CVD) device. The amorphous boron nitride layer 2 is used as a substrate, and the following are deposited on the surface: Silicon carbon nitride layer 1, Silicon Oxycarbide (NFDARC) layer 3, The metal mask (MHM) layer 4 and The silicon dioxide (MOC) layer 5, the M1 dielectric layer in the back-end copper interconnect structure is as shown in the attached Figure 4 shown.
[0058] Example 2
[0059] In the metal layer M1, tetramethylsilane and ammonia are used as precursors, helium is used as carrier gas, and a plasma enhanced chemical vapor deposition device is used to deposit on the device surface at 350°C. The silicon carbonitride layer 1 is used as a substrate, and boron nitride benzene is used as a precursor. An amorphous boron nitride layer 2 is formed by a one-step reaction at 350°C in a hydrogen flow through an inductively coupled plasma chemical vapor deposition device. The amorphous boron nitride layer 2 is used as a substrate, and the following are deposited on the surface: Silicon carbon nitride layer 1, Silicon oxycarbide layer 3, The metal mask layer 4 and The silicon dioxide layer 5 is formed to form the M1 dielectric layer in the back-end copper interconnect structure as shown in the attached Figure 4 shown.
[0060] Example 3
[0061] In the metal layer M6 (the sixth metal layer), tetramethylsilane and ammonia are used as precursors, helium is used as a carrier gas, and a plasma enhanced chemical vapor deposition device is used to deposit on the device surface at 400°C. The silicon carbonitride layer 1 is used as a substrate, and boron nitride benzene is used as a precursor. An amorphous boron nitride layer 2 is formed by a one-step reaction at 400°C in a hydrogen flow through an inductively coupled plasma chemical vapor deposition device. The amorphous boron nitride layer 2 is used as a substrate, and the following are deposited on the surface in sequence: Silicon carbon nitride layer 1, Silicon oxycarbide layer 3, The metal mask layer 4 and The silicon dioxide layer 5 is formed to form the M6 dielectric layer in the back-end copper interconnect structure as shown in the attached Figure 5 shown.
[0062] Example 4
[0063] In the metal layer M6, tetramethylsilane and ammonia are used as precursors, helium is used as carrier gas, and a plasma enhanced chemical vapor deposition device is used to deposit on the device surface at 350°C. The silicon carbonitride layer 1 is used as a substrate, and boron nitride benzene is used as a precursor. An amorphous boron nitride layer 2 is formed by a one-step reaction at 350°C in a hydrogen flow through an inductively coupled plasma chemical vapor deposition device. The amorphous boron nitride layer 2 is used as a substrate, and the following are deposited on the surface: Silicon carbon nitride layer 1, Silicon oxycarbide layer 3, The metal mask layer 4 and The silicon dioxide layer 5 forms the M6 dielectric layer in the back-end copper interconnect structure. Figure 5 shown.
[0064] Specific examples are used herein to illustrate the principles and implementation methods of the present application, and the embodiments are in a progressive relationship, each embodiment focuses on the differences from other embodiments, and the same and similar parts between the embodiments can be referred to each other. The description of the above embodiments is only used to help understand the method and core ideas of the present application. For ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.
[0065] It should also be noted that, in this specification, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "comprise", "include" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or equipment including the elements.
Claims
1. A method for preparing a copper interconnect dielectric layer structure, characterized in that: include: Depositing a protective layer on the surface of the substrate to protect the copper in the pre-deposited copper interconnect dielectric layer structure; An amorphous boron nitride film layer is deposited on the surface of the protective layer as an ultra-low dielectric constant dielectric layer to form the copper interconnect dielectric layer structure.
2. The method for preparing a copper interconnect dielectric layer structure according to claim 1, characterized in that: After depositing an amorphous boron nitride film layer on the surface of the protective layer as an ultra-low dielectric constant dielectric layer, the method further comprises: A silicon carbonitride layer, a silicon carbide layer, a metal mask layer and a silicon dioxide layer are sequentially deposited on the surface of the amorphous boron nitride film layer.
3. The method for preparing a copper interconnect dielectric layer structure according to claim 1, characterized in that: The protective layer is a silicon carbonitride layer.
4. The method for preparing a copper interconnect dielectric layer structure according to claim 3, characterized in that: The step of depositing a protective layer on the surface of the substrate comprises: Tetramethylsilane and ammonia are used as precursors and an inert gas is used as a carrier gas to deposit the silicon carbonitride layer on the surface of the substrate.
5. The method for preparing a copper interconnect dielectric layer structure according to claim 4, characterized in that: The method of using tetramethylsilane and ammonia as precursors and an inert gas as a carrier gas to deposit the silicon carbonitride layer on the surface of the substrate comprises: The silicon carbonitride layer is deposited on the surface of the substrate by using plasma enhanced chemical vapor deposition equipment, tetramethylsilane and ammonia as precursors and inert gas as carrier gas.
6. The method for preparing a copper interconnect dielectric layer structure according to any one of claims 1 to 5, characterized in that: Depositing an amorphous boron nitride film layer on the surface of the protective layer as an ultra-low dielectric constant dielectric layer includes: The amorphous boron nitride film layer is deposited on the surface of the protective layer as the ultra-low dielectric constant dielectric layer using boron nitride as a precursor in a hydrogen flow at a preset temperature.
7. The method for preparing a copper interconnect dielectric layer structure according to claim 6, characterized in that: Depositing the amorphous boron nitride film as the ultra-low dielectric constant layer on the surface of the protective layer using boron nitride as a precursor in a hydrogen flow at the preset temperature includes: The amorphous boron nitride film layer is deposited as the ultra-low dielectric constant dielectric layer on the surface of the protective layer using inductively coupled plasma chemical vapor deposition equipment at a preset temperature in a hydrogen flow using boron nitride as a precursor.
8. The method for preparing a copper interconnect dielectric layer structure according to claim 7, characterized in that: The preset temperature is 350° C. to 400° C., including both end values.
9. The method for preparing a copper interconnect dielectric layer structure according to claim 8, characterized in that: The thickness of the amorphous boron nitride film layer is greater than or equal to 10. A copper interconnect dielectric layer structure, characterized in that: include: A copper interconnect dielectric layer structure prepared by the method for preparing a copper interconnect dielectric layer structure according to any one of claims 1 to 9.