Flexible high electron mobility transistor and preparation method and application thereof

By combining the technology of indium phosphide-based high electron mobility transistor on a flexible substrate, the problem of preparing flexible electronic devices under high temperature conditions is solved, high cutoff frequency and bendable transistor preparation is achieved, and InP substrate is provided The secondary use solution simplifies the process and reduces costs.

CN119029027APending Publication Date: 2024-11-26INSTITUTE OF PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411125841.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to prepare high electron mobility transistors on flexible films that are not resistant to high temperatures, and the preparation process of flexible electronic devices is complicated and cannot be completed directly under high temperature conditions. It is necessary to prepare on an inorganic substrate and then transfer to the flexible substrate. .

Method used

The combination of indium phosphide-based high electron mobility transistor and flexible substrate is adopted, and the high cutoff frequency flexible indium phosphide-based high electron mobility transistor is prepared through molecular beam epitaxial and chemical vapor deposition of metal organic compounds. It also provides a secondary use method of InP substrate, simplifying the preparation process.

Benefits of technology

The efficient preparation of high electron mobility transistors on flexible substrates is achieved, which avoids temporary substrate size limitations, improves the degree of flexibility and stability of the device, and the InP substrate can be reused, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119029027A_ABST
    Figure CN119029027A_ABST
Patent Text Reader

Abstract

The invention provides a flexible high electron mobility transistor and a preparation method and application thereof. The flexible high-electron-mobility transistor comprises a flexible substrate, an n-type buffer layer, an n-type channel layer, an n-type isolation layer, a delta doping layer, a Schottky barrier layer, a corrosion cut-off layer, an n-type cap layer, a metal source electrode, a metal drain electrode, a metal gate electrode and a passivation layer which are sequentially arranged from bottom to top. According to the flexible indium phosphide-based high-electron-mobility transistor and the preparation method thereof, the indium phosphide-based high-electron-mobility transistor is combined with the flexible substrate, the flexible indium phosphide-based high-electron-mobility transistor which is high in cut-off frequency and can be bent is prepared, and the preparation method that the InP substrate can be used for the second time is provided. The preparation method is simpler and more convenient, an effective, feasible and low-cost scheme is provided for industrialization of semiconductor microelectronic devices on flexible substrates, and development of flexible inorganic microelectronic devices is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductors, and in particular relates to a flexible high electron mobility transistor, a preparation method and application thereof. Background Art

[0002] With the improvement of semiconductor device manufacturing technology and the development of integrated circuit technology, the demand for submillimeter wave and terahertz monolithic integrated circuits is increasing, and fields such as wireless communications, radio telescopes, satellite remote sensing and medical biological imaging are gradually entering the high-frequency era. Among them, indium phosphide (InP) materials have the characteristics of high electron mobility, large saturation drift velocity and large carrier surface density. Using gate, source, drain and other process technologies, indium phosphide-based field effect transistors can be made, such as heterojunction bipolar transistors, metal-oxide semiconductor field effect transistors, high electron mobility transistors, etc. Indium phosphide-based high electron mobility transistors have the characteristics of high cut-off frequency, high gain, low noise, low power consumption, high bandwidth, etc., and have important applications in high-speed integrated circuits, satellite communications, radio astronomy, high-resolution imaging arrays, low-temperature electronic information, and biomedical imaging.

[0003] Flexible electronic devices can be divided into flexible batteries, flexible sensors, flexible displays, flexible circuits and flexible light-emitting diodes according to their basic structure and use. In recent years, driven by the rapid development of low-dimensional nanostructures and materials, the application scenarios of flexible / stretchable electronic devices have become more flexible and have been widely used. Flexible electronic technology can be compatible with a variety of substrates to produce thinner and more flexible flexible electronic devices. Their small size, high stretchability and adaptability make them very suitable for medical, military, aviation, automotive and other fields. The progress of the preparation process of flexible electronic devices is gradually leading the development path of miniaturization, intelligence and integration in the post-Moore era. However, the preparation process of inorganic flexible electronic devices is more complicated and difficult than that of organic flexible electronic devices. Since the material structure is generally prepared under high temperature conditions (>300℃), it cannot be directly prepared on a flexible film that is not resistant to high temperatures. Therefore, it is necessary to prepare it on an inorganic substrate first, and then peel the flexible electronic device off the inorganic substrate and transfer it to a flexible film substrate. The commonly used method for preparing flexible electronic devices is to first bond a temporary substrate on the surface of the inorganic electronic device, then remove the inorganic substrate by chemical etching / mechanical stripping and finally transfer it to a flexible substrate.

[0004] Therefore, how to obtain a flexible high electron mobility transistor structure with good functions and not limited by the substrate size has become a difficult problem that needs to be solved urgently. Summary of the invention

[0005] Therefore, the purpose of the present invention is to overcome the defects in the prior art and provide a flexible high electron mobility transistor, a preparation method and application thereof. The present invention combines an indium phosphide-based high electron mobility transistor with a flexible substrate to obtain a high cut-off frequency, bendable, flexible indium phosphide-based high electron mobility transistor, and provides a preparation method for a secondary use of the InP substrate. The preparation method of the present invention is simpler and provides an effective, feasible and low-cost solution for the industrialization of semiconductor microelectronic devices on flexible substrates, which is conducive to promoting the development of flexible inorganic microelectronic devices.

[0006] Before describing the present invention, the terms used in this article are defined as follows:

[0007] The term "MBE" refers to: Molecular Beam Epitaxy.

[0008] The term "MOCVD" refers to: Metal-Organic Chemical Vapor Deposition, the English name is Metal-Organic Chemical Vapor Deposition.

[0009] The term "PECVD" means: Plasma Enhanced Chemical Vapor Deposition, the English name is Plasma Enhanced Chemical Vapor Deposition.

[0010] The term "ICP-PECVD" refers to: Inductively Coupled Plasma-Plasma Enhanced Chemical Vapor Deposition.

[0011] The term "RIE" means: reactive ion etching, also known as reactive ion etching in English.

[0012] The term "ICP-RIE" refers to: Inductively Coupled Plasma Reactive Ion Etching, the English name is Inductively Coupled Plasma Reactive Ion Etching.

[0013] The term "ALD" means: Atomic Layer Deposition.

[0014] The term "PDMS" refers to: polydimethylsiloxane, the English name is Polydimethylsiloxane.

[0015] The term "n-type" means that a semiconductor that mainly conducts electricity through electrons is an n-type semiconductor.

[0016] The term "p-type" means that a semiconductor that mainly conducts electricity through holes is called a p-type semiconductor.

[0017] The term "delta doping" means that the impurity atoms doped into the semiconductor are limited to one or several layers of semiconductor atomic planes. The mathematical delta function is usually used to describe this impurity distribution.

[0018] The term "InP" refers to: Indium Phosphide, whose English name is Indium Phosphide.

[0019] The term "ZEP" refers to a styrene methacrylate based electron beam positive resist.

[0020] The term "PMGI" refers to an electron beam positive resist with polydimethylglutarimide as the main component.

[0021] The term "MMA" refers to an electron beam positive resist based on methyl methacrylate.

[0022] The term "MAA" refers to an electron beam positive resist with methacrylic acid as the main component.

[0023] The term "PMMA" refers to an electron beam positive resist with polymethyl methacrylate as the main component.

[0024] The term "UV III" refers to an electron beam chemically amplified glue with a copolymer of 4-hydroxystyrene and butyl acrylate as the main component.

[0025] The term "PET" refers to polyethylene terephthalate, whose English name is polyethylene glycolterephthalate.

[0026] The term "PEN" refers to: polyethylene naphthalate, also known as Polyethylene naphtholate in English.

[0027] The term "PEEK" refers to: polyetheretherketone, the English name is Polyetheretherketone.

[0028] The term "PDMS" refers to: polydimethylsiloxane, the English name is Polydimethylsiloxane.

[0029] The term "PC" refers to: polycarbonate, the English name is Polycarbonate.

[0030] The term "PES" refers to: polyethersulfone, the English name is Polyether sulfone.

[0031] The term "PAR" refers to: Polyacrylate, polyarylate, the English name is Polyacrylate.

[0032] The term "PI" refers to: polyimide, the English name is Polyamide.

[0033] To achieve the above object, a first aspect of the present invention provides a flexible high electron mobility transistor, wherein the flexible high electron mobility transistor comprises:

[0034] Flexible substrate;

[0035] n-type buffer layer;

[0036] n-type channel layer;

[0037] n-type isolation layer;

[0038] δ-doped layer;

[0039] Schottky barrier layer;

[0040] Corrosion cut-off layer;

[0041] n-type cap layer;

[0042] Metal source electrode, metal drain electrode;

[0043] a metal gate electrode; and

[0044] Passivation layer.

[0045] According to the first aspect of the present invention, the flexible high electron mobility transistor is an indium phosphide-based transistor, and:

[0046] The material of the n-type buffer layer is selected from one or more of the following: InAlAs, GaAs, AlGaAs, preferably InAlAs or AlGaAs, most preferably InAlAs;

[0047] The material of the n-type channel layer is selected from one or more of the following: InGaAs, InAlAs, InAs, InSb, preferably selected from one or more of the following: InGaAs, InAlAs, InSb, more preferably InGaAs or InAlAs;

[0048] The material of the n-type isolation layer is selected from one or more of the following: InAlAs, AlSb, AlAs, preferably AlSb or InAlAs, most preferably InAlAs;

[0049] The material of the delta-doped layer is selected from one or more of the following: Si, SiC, SiGe, preferably Si or SiGe, most preferably Si;

[0050] The material of the Schottky barrier layer is selected from one or more of the following: InAlAs, InAlSb, AlSb, AlAs, InAlAsSb, preferably selected from one or more of the following: InAlAs, InAlAsSb, AlSb, most preferably InAlAs;

[0051] The material of the corrosion stop layer is selected from one or more of the following: InP, GaAs, InGaP, AlGaInP, preferably selected from one or more of the following: InP, GaAs, InGaP, more preferably InP or GaAs;

[0052] The material of the n-type cap layer is selected from one or more of the following: InAlAs, InGaAs, InAs, GaSb, preferably selected from one or more of the following: InAlAs, InGaAs, InAs, more preferably InAlAs or InGaAs;

[0053] The material of the metal source electrode and the metal drain electrode is selected from one or more of the following: Ti / Au, Ti / Pt / Au, Ni / Ge / Au, preferably selected from one or more of the following: Ti / Au, Ti / Pt / Au, Ni / Ge / Au, more preferably Ti / Au or Ti / Pt / Au;

[0054] The material of the metal gate electrode is selected from one or more of the following: Ti / Au, Ti / Pt / Au, Ni / Ge / Au, Ni / Au, Ni / Ge / Au / Ge / Ni, AuGeNiAu, preferably selected from one or more of the following: Ti / Au, Ti / Pt / Au, Ni / Ge / Au, more preferably Ti / Au or Ti / Pt / Au; and / or

[0055] The material of the passivation layer is selected from one or more of the following: Al2O3, Si x N y , SiO2, preferably Al2O3 or Si x N y ; wherein, the x preferably satisfies 2<x<4, more preferably satisfies 3≤x<4, and most preferably satisfies x to be 3; the y preferably satisfies 3<y<5, more preferably satisfies 4≤y<5, and most preferably satisfies y to be 4.

[0056] According to the first aspect of the present invention, the flexible high electron mobility transistor, wherein:

[0057] The material of the flexible substrate is selected from one or more of the following: a plastic substrate, a metal film substrate, an ultra-thin glass substrate, a paper substrate, a biocomposite film substrate, preferably selected from one or more of the following: a plastic substrate, a metal film substrate, an ultra-thin glass substrate, more preferably a plastic substrate or a metal film substrate;

[0058] The shape of the metal gate electrode is selected from one or more of the following: T-shaped, Y-shaped, Γ-shaped, preferably T-shaped or Y-shaped, and most preferably T-shaped;

[0059] The metal source electrode and the metal drain electrode are located on both sides of the metal gate electrode and are not connected; and / or

[0060] The metal gate electrode is located in the gate groove, and its bottom surface is connected to the surface of the corrosion stop layer to form a Schottky contact;

[0061] Preferably, the gate trenches are formed by corroding or etching the n-type cap layer to separate the gate trenches in space.

[0062] According to the first aspect of the present invention, the flexible high electron mobility transistor, wherein:

[0063] The material of the plastic substrate is selected from one or more of the following: semi-crystalline thermoplastic polymer, non-crystalline polymer, non-crystalline high glass transition temperature polymer, preferably selected from one or more of the following: semi-crystalline thermoplastic polymer, non-crystalline polymer, non-crystalline high glass transition temperature polymer; and / or

[0064] The material of the metal film substrate is selected from one or more of the following: copper, aluminum, iron, molybdenum copper, tungsten copper, chromium copper, preferably selected from one or more of the following: molybdenum copper, tungsten copper, chromium copper;

[0065] Preferably, the semi-crystalline thermoplastic polymer is selected from one or more of the following: PET, PEN, PEEK, PDMS, more preferably selected from one or more of the following: PET, PEEK, PDMS, further preferably PET or PDMS;

[0066] Preferably, the non-crystalline polymer is PC or PES non-crystalline thermoplastic, most preferably PES non-crystalline thermoplastic; and / or

[0067] Preferably, the non-crystalline high glass transition temperature polymer is PAR or PI.

[0068] The second aspect of the present invention provides a method for preparing the flexible high electron mobility transistor according to the first aspect, the method comprising the following steps:

[0069] (1) Preparing epitaxial wafers and performing table isolation;

[0070] (2) preparing a metal source electrode and a metal drain electrode;

[0071] (3) Electron beam exposure determines the morphology and size of the gate electrode metal;

[0072] (4) spatially isolating the n-type cap layer under the metal source electrode and the metal drain electrode and forming a gate groove;

[0073] (5) depositing gate electrode metal from bottom to top by electron beam evaporation, and performing metal stripping and photoresist removal after the gate electrode metal deposition is completed;

[0074] (6) Deposition of passivation layer;

[0075] (7) performing metal wiring and metal plate electrode overlap on the metal source electrode, the metal drain electrode and the metal gate electrode respectively;

[0076] (8) The device unit obtained in step (7) is transferred to a flexible substrate to obtain the flexible high electron mobility transistor.

[0077] According to the method of the second aspect of the present invention,

[0078] The step (1) comprises: epitaxially growing in sequence: a sacrificial layer, a buffer layer, an n-type channel layer, an n-type isolation layer, a delta-doped layer, a Schottky barrier layer, an etching stop layer, and an n-type cap layer on a recyclable substrate to obtain the epitaxial wafer, and isolating the epitaxial layers on the recyclable substrate into mutually non-conductive mesas by mesa isolation;

[0079] The step (2) comprises: preparing a pattern mask of the metal source electrode and the metal drain electrode on the n-type cap layer, and depositing metal to form an ohmic contact, thereby obtaining the metal source electrode and the metal drain electrode;

[0080] The step (3) comprises: growing a hard mask layer on the n-type cap layer, the metal source electrode and the metal drain electrode, and then performing electron beam exposure and development after spin coating electron beam glue on the hard mask layer;

[0081] In the step (5): the thickness of the gate electrode metal is 10 nm to 800 nm, preferably 15 nm to 700 nm, and more preferably 20 nm to 600 nm;

[0082] In the step (6): the deposition thickness of the passivation layer is 50 nm to 300 nm, preferably 80 nm to 200 nm, most preferably 100 nm; and / or

[0083] In the step (7), the metal of the metal wiring and the metal plate is selected from one or more of the following: Au, Ti / Au, Ti / Pt / Au, Ni / Ge / Au, Ni / Au, preferably selected from one or more of the following: Au, Ti / Au, Ti / Pt / Au, more preferably Au or Ti / Au;

[0084] Preferably, in step (1), the method of isolating the mesa is selected from one or more of the following: photolithography, laser direct writing, electron beam exposure, wet etching, RIE, ICP-RIE, more preferably selected from one or more of the following: wet etching, RIE, ICP-RIE, and most preferably wet etching;

[0085] Preferably, in step (2): the method for growing the metal is selected from one or more of the following: photolithography, electron beam evaporation, metal stripping, physical vapor deposition, chemical vapor deposition, laser direct writing, electron beam exposure, sputtering, ALD, preferably selected from one or more of the following: photolithography, electron beam evaporation, metal stripping, more preferably selected from one or more of the following: photolithography, electron beam evaporation, metal stripping; the method for preparing the graphic mask is selected from one or more of the following: ultraviolet exposure, laser direct writing, electron beam exposure, preferably ultraviolet exposure or laser direct writing, most preferably ultraviolet exposure; the thickness of the metal source electrode and the metal drain electrode is not less than 50nm, preferably not less than 40nm, more preferably not less than 30nm; and / or the spacing between the metal source electrode and the metal drain electrode is 1μm to 10μm, preferably 2μm to 5μm, more preferably 2μm to 3μm;

[0086] Preferably, in the step (3): the material of the hard mask layer is selected from one or more of the following: silicon dioxide, silicon nitride, aluminum oxide, preferably silicon dioxide or silicon nitride, most preferably silicon dioxide; and / or the electron beam glue is selected from one or more of the following: ZEP, PMGI, MMA, MAA, PMMA, UVⅢ, preferably selected from one or more of the following: ZEP, PMGI, PMMA, UVⅢ, more preferably ZEP or PMGI.

[0087] According to the method of the second aspect of the present invention, when the flexible high electron mobility transistor is an indium phosphide-based transistor, in the step (1):

[0088] The material of the sacrificial layer is selected from one or more of the following: InGaAs, InAlAs, InAs, preferably InGaAs or InAlAs, most preferably InGaAs;

[0089] The material of the buffer layer is selected from one or more of the following: indium phosphide, InAlAs, GaAs, InGaP, preferably indium phosphide or GaAs, most preferably indium phosphide; and / or

[0090] The recyclable substrate is a rigid material, preferably selected from one or more of the following: indium phosphide, GaAs, InSb, and most preferably indium phosphide.

[0091] According to the method of the second aspect of the present invention, the step (7) further comprises the following steps:

[0092] a) preparing a mask pattern on the surface of the epitaxial wafer, and etching the mask pattern down to the surface of the sacrificial layer to form a sacrificial layer channel;

[0093] b) depositing a passivation layer on the surface of the epitaxial wafer to cover the sidewalls of the mask pattern; and

[0094] c) etching the sacrificial layer to separate the high electron mobility transistor from the recyclable substrate and the buffer layer, and recovering the recyclable substrate for reuse.

[0095] According to the method of the second aspect of the present invention,

[0096] In the step a), the mask pattern is selected from one or more of the following: etching a square hole, etching a circular hole, corroding a circular hole, corroding a square hole, preferably etching a circular hole and / or corroding a square hole; and / or

[0097] In the step b), the deposition method of the passivation layer is selected from one or more of the following: PECVD, ICP-PECVD, ALD, preferably PECVD or ALD, most preferably PECVD.

[0098] The third aspect of the present invention provides the use of the flexible high electron mobility transistor described in the first aspect in the preparation of a flexible electronic device;

[0099] Preferably, the flexible electronic device is selected from one or more of the following: a flexible battery, a flexible sensor, a flexible display, a flexible circuit, a flexible light emitting diode, a flexible memory, and a flexible photodetector.

[0100] The present invention provides a flexible indium phosphide-based high electron mobility transistor and a preparation method thereof. The flexible indium phosphide-based high electron mobility transistor comprises the following arranged in order from bottom to top: a flexible substrate; an n-type InAlAs buffer layer; an n-type channel layer; an n-type InAlAs isolation layer; a delta doping layer; an InAlAs Schottky barrier layer; an InP corrosion cutoff layer; an n-type InAlAs cap layer; a metal source-drain electrode; a T-shaped metal gate electrode; and a passivation layer. The preparation method comprises growing an indium phosphide substrate epitaxial wafer, table isolation, source-drain electrode preparation, T-shaped metal gate preparation, gate groove preparation, passivation layer deposition, metal plate electrode overlap, stripping and removing the InP substrate and transferring it to a flexible substrate, so as to obtain a high cutoff frequency, bendable, flexible indium phosphide-based high electron mobility transistor, and provides a preparation method in which the InP substrate can be reused for a second time.

[0101] To achieve the above object, according to a preferred embodiment of the present invention, the flexible high electron mobility transistor of the first aspect of the present invention is a flexible indium phosphide-based high electron mobility transistor, and the flexible indium phosphide-based HEMT includes:

[0102] Flexible substrate;

[0103] n-type InAlAs buffer layer;

[0104] n-type channel layer;

[0105] n-type InAlAs isolation layer;

[0106] δ-doped layer;

[0107] InAlAs Schottky barrier layer;

[0108] InP etching cut-off layer;

[0109] n-type InAlAs cap layer;

[0110] Metal source and drain electrodes;

[0111] T-shaped metal gate electrode;

[0112] Passivation layer;

[0113] Wherein, the flexible indium phosphide-based high electron mobility transistor is an independent device and / or integrated in a circuit;

[0114] According to the first aspect of the present invention, the flexible indium phosphide-based high electron mobility transistor, wherein the flexible substrate is selected from one or more of the following: a plastic substrate, a metal film substrate, an ultra-thin glass substrate, a paper substrate, a biocomposite film substrate, preferably a plastic substrate or a metal film substrate; wherein:

[0115] Preferably, the plastic substrate is selected from one or more of the following: semi-crystalline thermoplastic polymers, non-crystalline polymers, non-crystalline high glass transition temperature polymers,

[0116] Further preferably, the semi-crystalline thermoplastic polymer is selected from one or more of the following: PET, PEN, PEEK, PDMS, the non-crystalline polymer is selected from one or more of the following: PC, PES non-crystalline thermoplastics, and / or the non-crystalline high glass transition temperature polymer is PAR and / or PI;

[0117] Preferably, the metal film substrate material is selected from one or more of the following: copper, aluminum, iron, molybdenum copper, tungsten copper, chromium copper,

[0118] According to the flexible indium phosphide-based high electron mobility transistor of the first aspect of the present invention, the upper source-drain metal electrode and the T-shaped metal gate electrode are selected from one or more of the following: Ti / Au, Ti / Pt / Au, Ni / Ge / Au, preferably Ti / Au or Ti / Pt / Au.

[0119] Preferably, the n-type channel layer is selected from one or more of the following: indium gallium arsenic, indium aluminum arsenic, and most preferably indium gallium arsenic;

[0120] The thickness of the metal thin film substrate material is preferably 1 to 200 μm, and more preferably 1 to 100 μm.

[0121] The δ-doped layer and the channel layer conduct electricity and provide electrons. The δ-doping thickness is only a few lattice constants in size, and the doping spectrum is similar to the Dirac function. It can be obtained by interrupting the channel layer growth process and simultaneously depositing impurities. The device prepared by this process has the characteristics of high charge density, short distance between the conductive channel and the gate electrode, high gate electrode breakdown voltage, high transconductance, etc.

[0122] The isolation layer is used to isolate the two-dimensional electron gas and the delta-doped layer, and its thickness should be such that it can completely isolate the two-dimensional electron gas and the delta-doped layer. The isolation layer material is selected from one or more of the following: InAlAs, AlSb, AlAs, preferably AlSb or InAlAs, and most preferably InAlAs.

[0123] The second aspect of the present invention provides a method for preparing the flexible indium phosphide-based high electron mobility transistor according to the first aspect, the method comprising the following steps:

[0124] (1) A sacrificial layer, an InP buffer layer, an InAlAs buffer layer, an InP buffer layer, an n-type channel layer, an n-type isolation layer, a delta-doped layer, an InAlAs Schottky barrier layer, an InP cutoff layer, and an n-type InAlAs cap layer are sequentially epitaxially grown on an InP substrate to obtain an InP-based epitaxial wafer.

[0125] (2) Performing mesa isolation on the epitaxial wafer obtained in step (1): Separating the epitaxial layer on the InP substrate into mutually non-conductive mesas.

[0126] (3) Prepare the source and drain metal electrodes of the device. Ti / Au, Ti / Pt / Au or Ni / Ge / Au metals are grown on the n-type InAlAs cap layer through processes such as photolithography, electron beam evaporation, and metal lift-off to form an ohmic contact. The contact resistance is optimized by adjusting the annealing temperature and annealing duration. The contact resistance is usually measured by the transmission line method. The size and spacing of the source and drain electrodes are controlled by the photolithography process, and the thickness of the metal electrode is controlled by electron beam evaporation.

[0127] (4) Electron beam exposure for T-gate preparation. This step has a great impact on device performance and yield. In this step, a SiO2 hard mask is grown using the PECVD / ICP-PECVD method to enhance the adhesion of the electron beam glue in the subsequent process and provide mechanical support for the subsequent T-gate preparation process. For the T-gate preparation of InP-based high electron mobility transistors, the morphology and size of the gate electrode metal are determined by the electron beam exposure conditions.

[0128] (5) After the morphology of the electron beam colloid is formed in step (4), an opening is formed on the SiO2 by a dry etching method, and then the cap layer under the source electrode and the drain electrode is spatially isolated by the wet etching method described in step (2), thereby forming a gate groove under the SiO2.

[0129] (6) T-type gate metal evaporation and stripping is to form gate contact. The gate metal is deposited from bottom to top by electron beam evaporation. After the gate metal deposition is completed, the metal stripping and photoresist removal are performed. Then, hydrofluoric acid wet etching is used to remove the SiO2 hard mask layer above the cap layer.

[0130] (7) Passivation layer deposition to improve device leakage characteristics and enhance device stability.

[0131] (8) Peripheral metal plate bonding: metal wiring and metal plate bonding are performed on the source, drain, and gate of the device respectively. The metal wiring and plate bonding are prepared by Ti / Au electron beam evaporation and metal stripping.

[0132] (9) Preparing a corrosion and / or etching hole mask pattern, and etching the corrosion and / or etching holes on the wafer surface down to the surface of the sacrificial layer to form a sacrificial layer channel.

[0133] (10) Deposition of SiN on the wafer surface x Passivation layer to coat the wafer surface and etch and / or etch the hole sidewalls;

[0134] (11) The sacrificial layer is corroded to separate the indium phosphide-based high electron mobility transistor from the InP substrate and the buffer layer, and the InP substrate is recovered for later use.

[0135] (12) The device unit peeled off in step (10) is transferred to a flexible substrate to obtain the flexible indium phosphide-based high electron mobility transistor.

[0136] In the step (1), the epitaxial growth method includes but is not limited to: MBE, MOCVD;

[0137] The mesa isolation method in step (2) is selected from one or more of the following: photolithography, laser direct writing, electron beam exposure, wet etching, RIE, ICP-RIE. Preferably, a wet etching method is used. Further preferably, the type and ratio of the solution can be H2O2:H3PO4:H2O (1:1:25) solution to etch the InGaAs epitaxial layer and the InAlAs epitaxial layer, and HCl:H2O (1.5:1) solution to etch the InP epitaxial layer.

[0138] In step (3), the source electrode and the drain electrode are rectangular in shape, and the size is preferably 8 μm×20 μm, 8 μm×30 μm, or 8 μm×40 μm. The spacing between the source electrode and the drain electrode is preferably 2 μm or 3 μm;

[0139] When dry etching is selected, the etching method is selected from one or more of the following: RIE, ICP-RIE, wherein when the ICP-RIE method is used for etching, the etching gas is selected from one or more of the following: Cl2, BCl3.

[0140] In the step (4), preferably, a preparation scheme is adopted in which three layers of ZEP / PMGI / ZEP glue of different thicknesses are spin-coated on the SiO2 hard mask layer and electron beam exposure is performed once. The spin-coating thickness of the ZEP / PMGI / ZEP three-layer glue, the electron beam exposure dose, and the development time determine the morphology and size of the gate.

[0141] In the step (5), the size of the opening of the SiO2 hard mask is consistent with the opening size of the lower layer of ZEP glue after development in step (4).

[0142] In the step (6): the gate electrode metal is selected from one or more of the following: Ti / Au, Ti / Pt / Au, Ni / Ge / Au, preferably Ti / Au or Ti / Pt / Au.

[0143] In the step (7): the passivation layer is selected from one or more of the following: Al2O3, SiN x, wherein x is the ratio of N ions to Si ions. The passivation layer is prepared by one or more methods selected from the following: PECVD, ICP-PECVD, ALD. Preferably, the Si3N4 (270°C) passivation layer can be deposited by PECVD or the Al2O3 (250°C) passivation layer can be deposited by ALD.

[0144] The gas used for the deposition is selected from one or more of the following: SiH4, NH3; the thickness of the deposition is 100 to 200 nm.

[0145] According to another preferred embodiment of the present invention, the flexible high electron mobility transistor of the first aspect of the present invention is a flexible indium phosphide-based high electron mobility transistor, and the flexible indium phosphide-based high electron mobility transistor includes:

[0146] Flexible substrate;

[0147] n-type InAlAs buffer layer;

[0148] n-type channel layer;

[0149] n-type InAlAs isolation layer;

[0150] δ-doped layer;

[0151] InAlAs Schottky barrier layer;

[0152] InP etching cut-off layer;

[0153] n-type InAlAs cap layer;

[0154] Metal source and drain electrodes;

[0155] T-shaped metal gate electrode;

[0156] Passivation layer.

[0157] According to the flexible InP-based high electron mobility transistor of the first aspect of the present invention, the flexible substrate comprises one or more of the following: a plastic substrate, a metal film substrate, an ultra-thin glass substrate, a paper substrate, or a bio-composite film substrate.

[0158] Preferably, the plastic substrate comprises a semi-crystalline thermoplastic polymer, a non-crystalline polymer and a non-crystalline high glass transition temperature polymer.

[0159] Preferably, the semi-crystalline thermoplastic polymer includes PET, PEN, PEEK and PDMS, the non-crystalline polymer includes PC, PES non-crystalline thermoplastic plastics, and the non-crystalline high glass transition temperature polymer includes PAR and PI.

[0160] Preferably, the metal film substrate material is selected from one or more of the following: copper, aluminum, iron, molybdenum copper, tungsten copper, chromium copper, and its thickness is 1 to 100 μm;

[0161] Preferably, the raw material of the transparent conductive electrode is any one of indium tin oxide, gold, silver, aluminum electrode, silver nanowire and conductive polymer film, and the thickness thereof is 2 to 100 nm.

[0162] The second aspect of the present invention provides a method for preparing the flexible indium phosphide-based high electron mobility transistor according to the first aspect, the method comprising the following steps:

[0163] An InGaAs sacrificial layer, an InP buffer layer, an InAlAs buffer layer, an n-type channel layer, a delta-doped layer, an InAlAs Schottky barrier layer, an InP cutoff layer, and an n-type InAlAs cap layer are sequentially epitaxially grown on a semi-insulating InP wafer substrate;

[0164] Preferably, the epitaxial growth method is selected from metal organic chemical vapor deposition and / or molecular beam epitaxy;

[0165] The wafer obtained by epitaxy is isolated from the mesa. The epitaxial layer on the InP substrate is separated into mutually non-conductive mesas. Preferably, the epitaxial layer mesa is a rectangle with a length of 30 μm, 40 μm, 50 μm and a width of 20 μm. Preferably, a wet etching method is adopted. Further preferably, the type and ratio of the solution can be H2O2:H3PO4:H2O (1:1:25) solution to etch the InGaAs epitaxial layer and the InAlAs epitaxial layer, and HCl:H2O (1.5:1) solution to etch the InP epitaxial layer.

[0166] (c) Prepare the source and drain metal electrodes of the device.

[0167] Preferably, the preparation method of the Ti / Au upper electrode layer is selected from electron beam evaporation and / or sputtering;

[0168] Preferably, the Ti / Au upper electrode layer is electroplated to a thickness of not less than 50 nm to obtain a Ti / Au upper electrode;

[0169] Preferably, the source electrode and drain electrode patterns are rectangular; the sizes are preferably 8μm×20μm, 8μm×30μm, 8μm×40μm.

[0170] The distance between the source electrode and the drain electrode is preferably 2 μm or 3 μm;

[0171] (d) Electron beam exposure of T-gate preparation; first, a SiO2 hard mask is grown by PECVD method, and then three layers of ZEP / PMGI / ZEP with thickness of 250nm / 600nm / 150nm are spin-coated on the SiO2 hard mask layer and an electron beam exposure is performed once.

[0172] (e) A dry etching method is used to form an opening on SiO2, and then a wet etching method is used to form a gate groove.

[0173] Preferably, the wet etching is to etch the InGaAs epitaxial layer and the InAlAs epitaxial layer with a H2O2:H3PO4:H2O (1:1:25) solution, and the InP epitaxial layer is etched with a HCl:H2O (1.5:1) solution. Preferably, the dry etching is to use ICP-RIE technology, and the etching gas is Cl2 / BCl3;

[0174] (f) Ti with a thickness of 150 nm and Au with a thickness of 600 nm are deposited from bottom to top by electron beam evaporation. After the gate metal deposition is completed, metal stripping and photoresist removal are performed. The SiO2 hard mask layer above the cap layer is removed by hydrofluoric acid wet etching.

[0175] (g) depositing a passivation layer on the wafer surface;

[0176] Preferably, the SiN x The preparation method of the passivation layer is selected from PECVD and / or ICP-PECVD, the deposition gas is SiH4 / NH3, and the deposition thickness is 200nm;

[0177] (h) forming a mask pattern by photolithography, and performing Ti / Au electron beam evaporation and metal stripping to prepare peripheral metal wiring and plate electrode overlap;

[0178] (i) preparing a corrosion and / or etching hole mask pattern, and etching the corrosion and / or etching hole on the surface of the wafer down to the surface of the sacrificial layer to form a sacrificial layer channel;

[0179] (j) Deposition of SiN on the wafer surface x Passivation layer to coat the corroded and / or etched hole sidewalls;

[0180] (k) etching the sacrificial layer using a wet etching technique to separate the indium phosphide-based high electron mobility transistor from the InP substrate and the buffer layer;

[0181] (l) Transferring the peeled device unit to a flexible substrate.

[0182] The preparation method of the indium phosphide-based epitaxial wafer includes but is not limited to MBE, MOCVD and other technologies;

[0183] The corrosion / etching technology includes but is not limited to wet corrosion technology, reactive ion etching technology, and inductively coupled plasma reactive ion etching;

[0184] The chemical vapor deposition technology includes but is not limited to plasma enhanced chemical vapor deposition technology and inductively coupled enhanced plasma chemical vapor deposition;

[0185] The flexible substrate includes one or more of the following: a plastic substrate, a metal film substrate, an ultra-thin glass substrate, a paper substrate, and a biocomposite film substrate;

[0186] The raw material of the transparent conductive electrode is any one of indium tin oxide, gold, silver, aluminum electrode, silver nanowire and conductive polymer film, and the thickness thereof is 2-100nm.

[0187] Flexible electronic technology is highly stretchable and adaptable, and can be compatible with a variety of substrates to produce thinner and more flexible electronic devices, which can be applied to medical, military, aviation, automotive and other fields. Flexible electronic devices are widely used in micro devices such as sensors, transistors, memory, light-emitting diodes, photodetectors, and solar cells. The progress of the preparation process of flexible electronic devices is gradually leading the development path of miniaturization, intelligence, and integration in the post-Moore era. Combining flexible electronic technology with indium phosphide-based high electron mobility transistors, flexible indium phosphide-based high electron mobility transistors with high cutoff frequency, high gain, low noise, low power consumption, and high bandwidth can be prepared. It is used in low-noise amplifiers, multipliers, multiplexers, triggers, etc. in high-speed integrated circuits; it has important applications in radar, satellite communications, radio astronomy, high-resolution imaging arrays, high-capacity wireless communications, atmospheric sensing, low-temperature electronic information, and biomedical imaging.

[0188] Most flexible photonics research is based on organic, polymer and / or amorphous semiconductor material systems. The challenge is the reliable transfer of large-area crystalline semiconductors, especially for those fragile material systems (e.g., gallium arsenide and indium phosphide). The preparation method of the present invention is applicable to a variety of flexible substrates, such as PET, PEN, ultra-thin glass, and metal films. In addition, the preparation method of the present invention uses PECVD / ICP-PECVD technology to prepare SiN to protect the sidewalls of the active layer. x Etching hole channels increase the material options for sacrificial layers and etch-stop layers, enabling the construction of a wider variety of microelectronic devices.

[0189] The flexible high electron mobility transistor and the preparation method thereof of the present invention may have but are not limited to the following beneficial effects:

[0190] 1. Adjustable size: The present invention prepares etching holes on the surface of the device wafer, first peels the device film off the inorganic substrate, and then transfers it to the flexible substrate, which is not limited by the size of the temporary transfer substrate. From the current manufacturing technology, it can be known that the device wafer of the present invention can adjust the preparation size from micron level to inch level.

[0191] 2. High degree of bendability: The present invention can peel off a large-size surface of 3mm×3mm on the device surface, ensuring that the flexible electronic device can be bent from a flat state to ±60 degrees and maintain effective performance.

[0192] 3. High cut-off frequency: High electron mobility materials including InP have the characteristics of large saturation drift velocity and large carrier surface density. High electron mobility field effect crystals based on high electron mobility materials including InP have the advantages of high cut-off frequency, high gain and low noise, and can be used in high-speed integrated circuits in low-noise amplifiers, multipliers, multiplexers, triggers, etc.

[0193] 4. Good device stability: In the preferred preparation method example of the present invention, before preparing the corrosion sacrificial layer, a dense anti-oxidation SiNx film is deposited by PECVD / ICP-PECVD technology to avoid oxidation of the device sidewalls and surface, thereby improving the stability of the device.

[0194] 5. High flexibility and compatibility: The preparation method of the present invention is applicable to a variety of flexible substrates, such as PET, PEN, ultra-thin glass, and metal films. In addition, the preferred preparation method example of the present invention uses PECVD / ICP-PECVD technology to prepare SiNx etching hole channels that protect the side walls of the active layer, which increases the material selection of the sacrificial layer and the etching stop layer, and can realize the construction of more microelectronic devices.

[0195] 6. Recyclable substrates can be reused: The recyclable substrates using InP materials as an example used in the preferred preparation method example of the present invention are thinned to a thickness of no more than 2 μm after multiple wet etchings. Compared with the original substrate thickness of more than 600 μm, the thinning ratio is less than 1%. The substrate surface can be polished and then used again. BRIEF DESCRIPTION OF THE DRAWINGS

[0196] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, wherein:

[0197] Figure 1 A flow chart of embodiment 1 of the present invention is shown.

[0198] Figure 2 A cross-sectional schematic diagram of the InP substrate described in Example 1 of the present invention is shown.

[0199] Figure 3A cross-sectional schematic diagram of the epitaxial growth structure on a wafer according to Example 1 of the present invention is shown.

[0200] Figure 4 A cross-sectional schematic diagram of the mesa after isolation in Example 1 of the present invention is shown.

[0201] Figure 5 A top view of the Ti / Au source-drain electrode prepared in Example 1 of the present invention is shown.

[0202] Figure 6 A cross-sectional schematic diagram of the preparation of Ti / Au source-drain electrodes according to Example 1 of the present invention is shown.

[0203] Figure 7 The cross-sectional schematic diagram of the ZEP / PMGI / ZEP three-layer electron beam gel during the preparation of the T-type grid in Example 1 of the present invention is shown.

[0204] Figure 8 The cross-sectional structure schematic diagram of the T-shaped gate metal after deposition and stripping in Embodiment 1 of the present invention is shown.

[0205] Fig. 9 The method for preparing SiN in Example 1 of the present invention is shown. x Schematic cross-section of the passivation layer.

[0206] Fig.10 A cross-sectional schematic diagram of a flexible indium phosphide-based high electron mobility transistor prepared in Example 1 of the present invention after removing the InP substrate and transferring to a PET substrate is shown.

[0207] Description of reference numerals:

[0208] 1. Recyclable substrate; 2. Sacrificial layer; 3. InP buffer layer; 4. InAlAs buffer layer; 5. n-type channel layer; 6. n-type isolation layer; 7. δ-doped layer; 8. Schottky barrier layer; 9. Corrosion stop layer; 10. n-type InAlAs cap layer; 11. n-type InGaAs cap layer; 12. Source and drain electrodes; 13. ZEP electron beam glue; 14. PMGI electron beam glue; 15. ZEP electron beam glue; 16. Metal T-type gate electrode; 17. Passivation layer; 18. Flexible substrate. DETAILED DESCRIPTION

[0209] The present invention will be further described below through specific embodiments in conjunction with the accompanying drawings. However, it should be understood that these embodiments are only used for more detailed and specific description and should not be understood as limiting the present invention in any form.

[0210] This section generally describes the materials and test methods used in the experiments of the present invention. Although many materials and operating methods used to achieve the purpose of the present invention are well known in the art, the present invention is still described as detailed as possible. It is clear to those skilled in the art that in the context, if not specifically stated, the materials and operating methods used in the present invention are well known in the art.

[0211] Example 1

[0212] This embodiment is an exemplary description of the indium phosphide-based flexible high electron mobility transistor and its preparation method of the present invention.

[0213] The cross-sectional schematic diagram of the flexible InP-based high electron mobility transistor of this embodiment is shown in FIG. Fig.10 shown.

[0214] The preparation method of the flexible indium phosphide-based high electron mobility transistor of this embodiment is as follows: Figure 1 As shown, it specifically includes the following steps:

[0215] S001: Growing epitaxial layers of InP-based high electron mobility transistors on semi-insulating InP substrates;

[0216] S002: Performing table isolation on the obtained epitaxial wafer;

[0217] S003: Preparation of Ti / Au source and drain electrodes for high electron mobility field effect transistors;

[0218] S004: Electron beam exposure of metal T-gate preparation;

[0219] S005: preparing a gate groove by wet etching to separate the source and drain of the device in space;

[0220] S006: electron beam evaporation deposition of Ti / Au metal to form a T-type grid, followed by metal stripping operation;

[0221] S007: Deposition of SiN x Passivation layer, covering the device surface;

[0222] S008: Metal wiring is overlapped on the source, drain and gate electrodes of the device respectively

[0223] S009: forming a mask by photolithography to prepare an etching hole with a size of 50 μm×50 μm;

[0224] S010: Deposition of SiN x The passivation layer covers the sidewalls of the corrosion holes;

[0225] S011: Wet etching of the InGaAs sacrificial layer to separate the InP-based high electron mobility transistor from the substrate;

[0226] S012: Transfer the device to a flexible substrate with PET evaporated on the surface.

[0227] Specifically:

[0228] (1) The structure required for the epitaxial growth described in S001 includes: a 500nm InGaAs sacrificial layer, a 50nm InP buffer layer, a 300nm InAlAs buffer layer, a 15nm n-type InGaAs channel layer, a 5nm InAlAs isolation layer, a Siδ doping layer, a 6nm InAlAs Schottky barrier layer, a 3nm InP cutoff layer, a 6nm n-type InAlAs cap layer, and a 25nm InGaAs cap layer.

[0229] InP substrate 1, InGaAs sacrificial layer 2, InP buffer layer 3, InAlAs buffer layer 4, InGaAs channel layer 5, InAlAs Schottky barrier layer 6, InP cutoff layer 7, n-type InGaAs cap layer 8, such as Figure 3 As shown. The material of the InP substrate 1 is a semi-insulating InP substrate with a crystal orientation, such as Figure 2 shown.

[0230] The required structure in this embodiment 1 is prepared by MBE epitaxial growth, wherein the size of the InP wafer is 2 inches. First, a 500nm InGaAs sacrificial layer 2 is grown on a semi-insulating InP wafer substrate, and then a 50nm InP buffer layer, a 300nm InAlAs buffer layer, a 15nm n-type InGaAs channel layer, a 5nm InAlAs isolation layer, a Siδ doping layer, a 6nmInAlAs Schottky barrier layer, a 3nm InP cutoff layer, a 6nm n-type InAlAs cap layer, and a 25nm InGaAs cap layer are grown in sequence.

[0231] (2) In S002, the mesa isolation includes using a wet etching method to separate the epitaxial layer on the InP substrate into mutually non-conductive mesas. The InGaAs epitaxial layer and the InAlAs epitaxial layer are etched using a H2O2:H3PO4:H2O (1:1:25) solution, and the InP epitaxial layer is etched using a HCl:H2O (1.5:1) solution. The mesa structure schematic diagram is as follows: Figure 4 shown.

[0232] (3) Preparation of Ti / Au source and drain electrodes as described in S003. In this embodiment 1, the mask of the electrode pattern is prepared by ultraviolet exposure technology. The electrode shape and size are a 20μm×8μm rectangle. The spacing between the metal source electrode and the metal drain electrode is 2μm. The electron beam evaporation technology is used to evaporate and prepare the Ti / Au top electrode. Its electrode structure is Ti / Au (20nm / 100nm). Figure 6 shown. Figure 5 Schematic diagram of top view for preparing Ti / Au upper electrode layer unit.

[0233] (4) In S004, 15nm SiO2 is first grown on the wafer surface by PEVCD method. Then, three layers of ZEP / PMGI / ZEP with thickness of 250nm / 600nm / 200nm are spin-coated on the SiO2 hard mask layer and electron beam exposure is performed once. The line width of the electron beam exposure is 100nm and the exposure metering is 450μC / cm 2 The schematic diagram of the morphology of the three-layer ZEP / PMGI / ZEP adhesive after development is shown in the figure. Figure 7 shown.

[0234] (5) Prepare the gate groove by wet etching as described in S005. First, form an opening on SiO2 by dry etching, then use the wet etching method described in step (2) to spatially isolate the n-type cap layer under the source electrode and the drain electrode, and form a gate groove under SiO2. Use H2O2:H3PO4:H2O (1:1:25) solution to etch the InGaAs epitaxial layer and InAlAs epitaxial layer, and the etching time is 60s.

[0235] (6) Preparation of the metal T-shaped gate electrode described in S006: First, RIE etching technology is used to etch a hole on the SiO2 below the lower ZEP glue in S005, and the etching gas is CF4 / O2. The Ti / Au metal system with a thickness of 20nm / 600nm is deposited by electron beam evaporation to form a gate contact. After the gate metal deposition is completed, the metal is stripped and the photoresist is removed. Then, hydrofluoric acid wet etching is used to remove the SiO2 hard mask layer above the cap layer. Its structural cross-section is as follows: Figure 8 shown.

[0236] (7) The preparation method of the passivation layer described in S007 is to deposit a 100 nm thick Si3N4 passivation layer at 270°C using PECVD.

[0237] (8) For the peripheral metal wiring described in S008, a 2μm×2μm mask pattern is prepared on the surface of Si3N4 in S007 by UV lithography, respectively, above the source, drain, and gate, and then a hole is etched on Si3N4 by RIE. Finally, a 100nm thick Au pattern is deposited by electron beam evaporation to realize the peripheral metal wiring.

[0238] (9) In S009, a 30 μm×30 μm square etched hole pattern is prepared by using UV exposure technology. Combined with RIE etching technology, the surface of the InGaAs sacrificial layer is etched to form a sacrificial layer channel, and the etching gas is CF4 / O2.

[0239] (10) The Si3N4 passivation layer is prepared as described in S010, and Si3N4 is deposited by PECVD technology, wherein the deposition gas is SiH4 / NH3, and the coating thickness of the corrosion hole sidewall is 100nm.

[0240] (11) Separating the indium phosphide-based high electron mobility transistor and the substrate as described in S011, this embodiment uses a wet etching technique to etch the sacrificial layer. Use an etching solution of H2SO4:H2O2:H2O in a ratio of 1:8:120, and the etching time is 6 to 10 hours. Recover the InP substrate for later use.

[0241] (12) The device unit peeled off in the step is transferred to a flexible substrate to obtain the flexible indium phosphide-based high electron mobility transistor.

[0242] Embodiments 2 to 6

[0243] This embodiment is another exemplary description of the indium phosphide-based flexible high electron mobility transistor and its preparation method of the present invention.

[0244] The preparation methods of Examples 2 to 6 are the same as those of Example 1, except for Table 1.

[0245] Table 1 Flexible high electron mobility transistor of the present invention

[0246]

[0247]

[0248]

[0249]

[0250] Example 7

[0251] This embodiment is used to illustrate the effect of the indium phosphide-based flexible high electron mobility transistor of the present invention.

[0252] The DC gain of the flexible high electron mobility transistor prepared in Examples 1 to 6 is defined as the rate of change of the source drain current with the gate voltage change when the drain voltage bias is constant. The DC gain is an important parameter for calibrating the gate voltage's modulation capability on the source drain current, and its size is determined by the metal gate electrode length, metal gate-channel layer dielectric constant, metal gate width, metal gate-channel layer distance, and related parasitic impedance defined in the device preparation steps S003 to S006. The cutoff frequency of the flexible high electron mobility transistor is the maximum operating frequency at which the transistor can generate a DC gain, which is proportional to the peak DC gain and inversely proportional to the sum of the metal gate electrode-metal source electrode capacitance and the metal gate electrode-metal drain electrode capacitance. Its size is determined by the metal gate electrode length, metal gate-channel layer dielectric constant, metal gate width, metal gate-channel layer distance, and passivation layer dielectric constant and thickness defined in the device preparation steps S003 to S006.

[0253] The flexible substrates PET, PDMS, and PAR used in the flexible high electron mobility transistors prepared in Examples 1 to 6 are relatively easy to obtain and have a small thickness, which is suitable for large-angle bending. The main structure of the flexible high electron mobility transistor is mainly composed of an n-type buffer layer and a passivation layer with a large difference in elastic modulus. Factors affecting the performance of the flexible high electron mobility transistor in a bent state include: the radius of curvature of the flexible substrate bending, the total thickness of the epitaxial layer of the high electron mobility transistor, and the types of n-type buffer layer and passivation layer materials. For epitaxial layers with a total thickness of more than 500nm, the mechanisms of device failure due to bending include: cracking, slippage, and delamination; the mode of the failure mechanism is determined by the maximum value between the fracture stress, shear stress, and peeling stress of each layer.

[0254] After testing, the flexible high electron mobility transistors prepared in Examples 1 to 6 have a large degree of bendability, and a large surface of 3mm×3mm can be peeled off on the device surface, ensuring that the flexible electronic device can be bent from a flat state to ±60 degrees and maintain effective performance. At the same time, the recyclable substrates of the flexible high electron mobility transistors prepared in Examples 1 to 6 can be reused. After multiple tests by the inventors, it is confirmed that the recyclable substrates, such as InP materials, are thinned to a thickness of no more than 2μm after multiple wet etchings. Compared with the original substrate thickness of more than 600μm, the thinning ratio is less than 1%, and the substrate surface can be polished and reused.

[0255] Based on the above, the indium phosphide-based flexible high electron mobility transistor of the present invention can adjust the preparation size from the micron level to the inch level, can be bent to a large extent while maintaining effective performance, has the advantages of high cutoff frequency, high gain, and low noise, and has good device stability and high flexibility and compatibility, and can realize the construction of more types of microelectronic devices.

[0256] Although the effects of some embodiments are shown above, those skilled in the art should understand that according to the concept of the present invention, the aforementioned other embodiments without specific effects or other technical solutions of the present invention not shown in the embodiments can also achieve the following technical effects stated in the invention content section that are equivalent to the embodiments:

[0257] 1. Adjustable size: The present invention prepares etching holes on the surface of the device wafer, first peels the device film off the inorganic substrate, and then transfers it to the flexible substrate, which is not limited by the size of the temporary transfer substrate. From the current manufacturing technology, it can be known that the device wafer of the present invention can adjust the preparation size from micron level to inch level.

[0258] 2. High degree of bendability: The present invention can peel off a large-size surface of 3mm×3mm on the device surface, ensuring that the flexible electronic device can be bent from a flat state to ±60 degrees and maintain effective performance.

[0259] 3. High cut-off frequency: High electron mobility materials including InP have the characteristics of large saturation drift velocity and large carrier surface density. High electron mobility field effect crystals based on high electron mobility materials including InP have the advantages of high cut-off frequency, high gain and low noise, and can be used in high-speed integrated circuits in low-noise amplifiers, multipliers, multiplexers, triggers, etc.

[0260] 4. Good device stability: In the preferred preparation method example of the present invention, before preparing the corrosion sacrificial layer, a dense anti-oxidation SiNx film is deposited by PECVD / ICP-PECVD technology to avoid oxidation of the device sidewalls and surface, thereby improving the stability of the device.

[0261] 5. High flexibility and compatibility: The preparation method of the present invention is applicable to a variety of flexible substrates, such as PET, PEN, ultra-thin glass, and metal films. In addition, the preferred preparation method example of the present invention uses PECVD / ICP-PECVD technology to prepare SiNx etching hole channels that protect the side walls of the active layer, which increases the material selection of the sacrificial layer and the etching stop layer, and can realize the construction of more microelectronic devices.

[0262] 6. Recyclable substrates can be reused: The recyclable substrates using InP materials as an example used in the preferred preparation method example of the present invention are thinned to a thickness of no more than 2 μm after multiple wet etchings. Compared with the original substrate thickness of more than 600 μm, the thinning ratio is less than 1%. The substrate surface can be polished and then used again.

[0263] Although the present invention has been described to a certain extent, it is obvious that appropriate changes in various conditions can be made without departing from the spirit and scope of the present invention. It is understood that the present invention is not limited to the embodiments described, but belongs to the scope of the claims, which includes equivalent replacements of each factor described.

Claims

1. A flexible high electron mobility transistor, characterized in that: The flexible high electron mobility transistor includes: Flexible substrate; n-type buffer layer; n-type channel layer; n-type isolation layer; δ-doped layer; Schottky barrier layer; Corrosion cut-off layer; n-type cap layer; Metal source electrode, metal drain electrode; Metal gate electrode; and Passivation layer.

2. The flexible high electron mobility transistor according to claim 1, characterized in that: The flexible high electron mobility transistor is an indium phosphide-based transistor, and: The material of the n-type buffer layer is selected from one or more of the following: InAlAs, GaAs, AlGaAs, preferably InAlAs or AlGaAs, most preferably InAlAs; The material of the n-type channel layer is selected from one or more of the following: InGaAs, InAlAs, InAs, InSb, preferably selected from one or more of the following: InGaAs, InAlAs, InSb, more preferably InGaAs or InAlAs; The material of the n-type isolation layer is selected from one or more of the following: InAlAs, AlSb, AlAs, preferably AlSb or InAlAs, most preferably InAlAs; The material of the delta-doped layer is selected from one or more of the following: Si, SiC, SiGe, preferably Si or SiGe, most preferably Si; The material of the Schottky barrier layer is selected from one or more of the following: InAlAs, InAlSb, AlSb, AlAs, InAlAsSb, preferably selected from one or more of the following: InAlAs, InAlAsSb, AlSb, most preferably InAlAs; The material of the corrosion stop layer is selected from one or more of the following: InP, GaAs, InGaP, AlGaInP, preferably selected from one or more of the following: InP, GaAs, InGaP, more preferably InP or GaAs; The material of the n-type cap layer is selected from one or more of the following: InAlAs, InGaAs, InAs, GaSb, preferably selected from one or more of the following: InAlAs, InGaAs, InAs, more preferably InAlAs or InGaAs; The material of the metal source electrode and the metal drain electrode is selected from one or more of the following: Ti / Au, Ti / Pt / Au, Ni / Ge / Au, preferably selected from one or more of the following: Ti / Au, Ti / Pt / Au, Ni / Ge / Au, more preferably Ti / Au or Ti / Pt / Au; The material of the metal gate electrode is selected from one or more of the following: Ti / Au, Ti / Pt / Au, Ni / Ge / Au, Ni / Au, Ni / Ge / Au / Ge / Ni, AuGeNiAu, preferably selected from one or more of the following: Ti / Au, Ti / Pt / Au, Ni / Ge / Au, more preferably Ti / Au or Ti / Pt / Au; and / or The material of the passivation layer is selected from one or more of the following: Al2O3, Si x N y , SiO2, preferably Al2O3 or Si x N y ; wherein, the x preferably satisfies 2<x<4, more preferably satisfies 3≤x<4, and most preferably satisfies x to be 3; the y preferably satisfies 3<y<5, more preferably satisfies 4≤y<5, and most preferably satisfies y to be 4.

3. The flexible high electron mobility transistor according to claim 1 or 2, characterized in that: The material of the flexible substrate is selected from one or more of the following: a plastic substrate, a metal film substrate, an ultra-thin glass substrate, a paper substrate, a biocomposite film substrate, preferably selected from one or more of the following: a plastic substrate, a metal film substrate, an ultra-thin glass substrate, more preferably a plastic substrate or a metal film substrate; The shape of the metal gate electrode is selected from one or more of the following: T-shaped, Y-shaped, Γ-shaped, preferably T-shaped or Y-shaped, and most preferably T-shaped; The metal source electrode and the metal drain electrode are located on both sides of the metal gate electrode and are not connected; and / or The metal gate electrode is located in the gate groove, and its bottom surface is connected to the surface of the corrosion stop layer to form a Schottky contact; Preferably, the gate trenches are formed by corroding or etching the n-type cap layer to separate the gate trenches in space.

4. The flexible high electron mobility transistor according to claim 3, characterized in that: The material of the plastic substrate is selected from one or more of the following: semi-crystalline thermoplastic polymer, non-crystalline polymer, non-crystalline high glass transition temperature polymer, preferably selected from one or more of the following: semi-crystalline thermoplastic polymer, non-crystalline polymer, non-crystalline high glass transition temperature polymer; and / or The material of the metal film substrate is selected from one or more of the following: copper, aluminum, iron, molybdenum copper, tungsten copper, chromium copper, preferably selected from one or more of the following: molybdenum copper, tungsten copper, chromium copper; Preferably, the semi-crystalline thermoplastic polymer is selected from one or more of the following: PET, PEN, PEEK, PDMS, more preferably selected from one or more of the following: PET, PEEK, PDMS, further preferably PET or PDMS; Preferably, the non-crystalline polymer is PC or PES non-crystalline thermoplastic, most preferably PES non-crystalline thermoplastic; and / or Preferably, the non-crystalline high glass transition temperature polymer is PAR or PI.

5. A method for preparing a flexible high electron mobility transistor according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: (1) Preparing epitaxial wafers and performing table isolation; (2) preparing a metal source electrode and a metal drain electrode; (3) Electron beam exposure determines the morphology and size of the gate electrode metal; (4) spatially isolating the n-type cap layer under the metal source electrode and the metal drain electrode and forming a gate groove; (5) depositing gate electrode metal from bottom to top by electron beam evaporation, and performing metal stripping and photoresist removal after the gate electrode metal deposition is completed; (6) Deposition of passivation layer; (7) performing metal wiring and metal plate electrode overlap on the metal source electrode, the metal drain electrode and the metal gate electrode respectively; (8) The device unit obtained in step (7) is transferred to a flexible substrate to obtain the flexible high electron mobility transistor.

6. The method according to claim 5, characterized in that: The step (1) comprises: epitaxially growing in sequence: a sacrificial layer, a buffer layer, an n-type channel layer, an n-type isolation layer, a delta-doped layer, a Schottky barrier layer, an etching stop layer, and an n-type cap layer on a recyclable substrate to obtain the epitaxial wafer, and isolating the epitaxial layers on the recyclable substrate into mutually non-conductive mesas by mesa isolation; The step (2) comprises: preparing a pattern mask of the metal source electrode and the metal drain electrode on the n-type cap layer, and depositing metal to form an ohmic contact, thereby obtaining the metal source electrode and the metal drain electrode; The step (3) comprises: growing a hard mask layer on the n-type cap layer, the metal source electrode and the metal drain electrode, and then performing electron beam exposure and development after spin coating electron beam glue on the hard mask layer; In the step (5): the thickness of the gate electrode metal is 10 nm to 800 nm, preferably 15 nm to 700 nm, and more preferably 20 nm to 600 nm; In the step (6): the deposition thickness of the passivation layer is 50 nm to 300 nm, preferably 80 nm to 200 nm, most preferably 100 nm; and / or In the step (7), the metal of the metal wiring and the metal plate is selected from one or more of the following: Au, Ti / Au, Ti / Pt / Au, Ni / Ge / Au, Ni / Au, preferably selected from one or more of the following: Au, Ti / Au, Ti / Pt / Au, more preferably Au or Ti / Au; Preferably, in step (1), the method of isolating the mesa is selected from one or more of the following: photolithography, laser direct writing, electron beam exposure, wet etching, RIE, ICP-RIE, more preferably selected from one or more of the following: wet etching, RIE, ICP-RIE, and most preferably wet etching; Preferably, in step (2): the method for growing the metal is selected from one or more of the following: photolithography, electron beam evaporation, metal stripping, physical vapor deposition, chemical vapor deposition, laser direct writing, electron beam exposure, sputtering, ALD, preferably selected from one or more of the following: photolithography, electron beam evaporation, metal stripping, more preferably selected from one or more of the following: photolithography, electron beam evaporation, metal stripping; the method for preparing the graphic mask is selected from one or more of the following: ultraviolet exposure, laser direct writing, electron beam exposure, preferably ultraviolet exposure or laser direct writing, most preferably ultraviolet exposure; the thickness of the metal source electrode and the metal drain electrode is not less than 50nm, preferably not less than 40nm, more preferably not less than 30nm; and / or the spacing between the metal source electrode and the metal drain electrode is 1μm to 10μm, preferably 2μm to 5μm, more preferably 2μm to 3μm; Preferably, in the step (3): the material of the hard mask layer is selected from one or more of the following: silicon dioxide, silicon nitride, aluminum oxide, preferably silicon dioxide or silicon nitride, most preferably silicon dioxide; and / or the electron beam glue is selected from one or more of the following: ZEP, PMGI, MMA, MAA, PMMA, UVⅢ, preferably selected from one or more of the following: ZEP, PMGI, PMMA, UVⅢ, more preferably ZEP or PMGI.

7. The method according to claim 6, characterized in that When the flexible high electron mobility transistor is an indium phosphide-based transistor, in the step (1): The material of the sacrificial layer is selected from one or more of the following: InGaAs, InAlAs, InAs, preferably InGaAs or InAlAs, most preferably InGaAs; The material of the buffer layer is selected from one or more of the following: indium phosphide, InAlAs, GaAs, InGaP, preferably indium phosphide or GaAs, most preferably indium phosphide; and / or The recyclable substrate is a rigid material, preferably selected from one or more of the following: indium phosphide, GaAs, InSb, and most preferably indium phosphide.

8. The method according to any one of claims 5 to 7, characterized in that The step (7) further includes the following steps: a) preparing a mask pattern on the surface of the epitaxial wafer, and etching the mask pattern down to the surface of the sacrificial layer to form a sacrificial layer channel; b) depositing a passivation layer on the surface of the epitaxial wafer to cover the sidewalls of the mask pattern; and c) etching the sacrificial layer to separate the high electron mobility transistor from the recyclable substrate and the buffer layer, and recovering the recyclable substrate for reuse.

9. The method according to any one of claims 5 to 8, characterized in that: In the step a), the mask pattern is selected from one or more of the following: etching a square hole, etching a circular hole, corroding a circular hole, corroding a square hole, preferably etching a circular hole and / or corroding a square hole; and / or In the step b), the deposition method of the passivation layer is selected from one or more of the following: PECVD, ICP-PECVD, ALD, preferably PECVD or ALD, most preferably PECVD.

10. Use of the flexible high electron mobility transistor according to any one of claims 1 to 4 in preparing flexible electronic devices; Preferably, the flexible electronic device is selected from one or more of the following: a flexible battery, a flexible sensor, a flexible display, a flexible circuit, a flexible light emitting diode, a flexible memory, and a flexible photodetector.