Flexible solar cell module and preparation method thereof, and flexible solar cell

The preparation of metal layers and evaporation technology is formed by magnetron sputtering in a mixture of argon and nitrogen, and the perovskite active layer is formed by combining single source evaporation to form a flexible perovskite solar cell. The accumulation of defects and material brittleness problems during preparation improves the power conversion efficiency and stability of the battery.

CN119031807APending Publication Date: 2024-11-26SUZHOU GUOXIAN INNOVATION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411151143.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Flexible perovskite solar cells have defect accumulation and material brittleness problems during the preparation process, which affects their long-term stability and power conversion efficiency. Traditional transparent electrode materials are costly and fragile.

Method used

The metal layer is prepared by magnetron sputtering in a mixture of argon and nitrogen, and the oxide/metal/oxide electrode is prepared in combination with evaporation technology, which increases the wettability of the metal layer and the density of the electrode, reduces the surface resistance, and A high-quality perovskite active layer is formed by single source evaporation, avoiding the influence of water and oxygen.

Benefits of technology

The power conversion efficiency of perovskite solar cells is improved, the flexibility and long-term stability of the electrode are enhanced, the preparation cost is reduced, and the power conversion efficiency is maintained after multiple bends.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031807A_ABST
    Figure CN119031807A_ABST
Patent Text Reader

Abstract

The invention provides a flexible solar cell module and a preparation method thereof, and a flexible solar cell. The preparation method of the flexible solar cell module comprises the following steps: providing a substrate; a first oxide layer is prepared on one side of the substrate, in mixed gas of argon and nitrogen, a metal layer is prepared on the side, away from the substrate, of the first oxide layer through magnetron sputtering, a second oxide layer is prepared on the side, away from the substrate, of the metal layer, and the first oxide layer, the metal layer and the second oxide layer form a first electrode layer; preparing a first transmission layer on one side, far away from the substrate, of the first electrode layer; preparing a perovskite active layer on one side, far away from the substrate, of the first transmission layer; preparing a second transmission layer on one side, far away from the substrate, of the perovskite active layer; and preparing a second electrode layer on one side, far away from the substrate, of the second transmission layer. According to the technical scheme, the power conversion efficiency of the solar cell can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular to a flexible solar cell assembly and a preparation method thereof, and a flexible solar cell. Background Art

[0002] With the development of technology and the continuous growth of human needs, it is particularly important to develop smaller, lighter and thinner energy storage devices. Flexible solar cells, especially flexible perovskite solar cells, have the characteristics of light weight and bendability, and have gradually become one of the research hotspots at this stage.

[0003] However, flexible perovskite solar cells still face some preparation difficulties, which hinder the widespread application of flexible perovskite solar cells. Summary of the invention

[0004] In order to solve the above problems, the embodiments of the present application provide a method for preparing a flexible solar cell module, a flexible solar cell module and a flexible solar cell.

[0005] In a first aspect, an embodiment of the present application provides a method for preparing a flexible solar cell module, comprising: providing a substrate; preparing a first oxide layer on one side of the substrate, preparing a metal layer by magnetron sputtering on a side of the first oxide layer away from the substrate in a mixture of argon and nitrogen, and preparing a second oxide layer on a side of the metal layer away from the substrate, wherein the first oxide layer, the metal layer, and the second oxide layer constitute a first electrode layer; preparing a first transmission layer on a side of the first electrode layer away from the substrate; preparing a perovskite active layer on a side of the first transmission layer away from the substrate; preparing a second transmission layer on a side of the perovskite active layer away from the substrate; and preparing a second electrode layer on a side of the second transmission layer away from the substrate.

[0006] In combination with the first aspect, in a mixture of argon and nitrogen, a metal layer is prepared on a side of the first oxide layer away from the substrate by magnetron sputtering, including: the gas pressure of the mixture of argon and nitrogen is 1 to 8 mTorr, the volume proportion of nitrogen in the mixture of argon and nitrogen is 0.01% to 1%, preferably, the sputtering power is 100 to 500 W; preferably, the deposition rate of the metal layer is Preferably, the material of the metal layer is silver; preferably, the thickness of the metal layer is 1-12 nm.

[0007] In combination with the first aspect, preparing a first oxide layer on one side of the substrate includes: evaporating a material for the first oxide layer on one surface of the substrate under vacuum to obtain the first oxide layer; preferably, the evaporation is electron beam evaporation; preferably, the vacuum degree is 10 -3 ~10 -4 Pa, the evaporation rate is Preferably, the material of the first oxide layer includes at least one of zinc oxide, tungsten oxide, and molybdenum oxide; preferably, the thickness of the first oxide layer is 5 to 50 nm; and / or, preparing the second oxide layer on the side of the metal layer away from the substrate comprises: evaporating the material of the second oxide on the surface of the metal layer away from the substrate under vacuum to obtain the second oxide layer; preferably, the evaporation is electron beam evaporation; preferably, the vacuum degree of the vacuum is 10 -3 ~10 - 4 Pa, the evaporation rate is Preferably, the material of the second oxide layer includes at least one of zinc oxide, tungsten oxide and molybdenum oxide; preferably, the thickness of the second oxide layer is 5-50 nm.

[0008] In combination with the first aspect, the perovskite active layer includes at least two layers of perovskite raw material layers, and the perovskite active layer is prepared on the side of the first transmission layer away from the substrate, comprising: sequentially evaporating at least two layers of perovskite raw material layers on the surface of the first transmission layer away from the substrate, and then annealing to obtain the perovskite active layer; preferably, the evaporation is thermal evaporation, and the evaporation rate is Preferably, the raw material layer of each perovskite layer is prepared by single-source evaporation; preferably, the annealing temperature is 100-300°C, and the annealing time is 2-20 min; preferably, the raw materials of the perovskite include at least one of cesium iodide, methylamine iodide, and formamidine iodide and lead iodide; preferably, the thickness of the raw material layer of each perovskite layer is 0.5nm-30nm, and the thickness of the perovskite active layer is 200-800nm.

[0009] In combination with the first aspect, a first transmission layer is prepared on a side of the first electrode layer away from the substrate, comprising: in a mixture of argon and oxygen, sputtering a material of the first transmission layer on a surface of the first electrode layer away from the substrate to obtain the first transmission layer; preferably, the gas pressure of the mixture of argon and oxygen is 1 to 8 mTorr, the volume proportion of oxygen in the mixture of argon and oxygen is 0.01% to 2%, preferably, the sputtering power is 100 to 500 W; preferably, the deposition rate of the first transmission layer is Preferably, the material of the first transmission layer is nickel oxide; preferably, the thickness of the first transmission layer is 5-40 nm.

[0010] In combination with the first aspect, a second transport layer is prepared on a side of the perovskite active layer away from the substrate, comprising: evaporating a material of the second transport layer on a surface of the perovskite active layer away from the substrate to obtain the second transport layer; preferably, the evaporation is thermal evaporation, and the evaporation rate is Preferably, the material of the second transmission layer includes at least two of fullerene, fullerene derivatives, phenyl C61 butyric acid methyl ester, and 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline; preferably, the thickness of the second transmission layer is 10 to 60 nm.

[0011] In combination with the first aspect, preparing a second electrode layer on a side of the second transmission layer away from the substrate comprises: evaporating a material of the second electrode layer on a surface of the second transmission layer away from the substrate to obtain the second electrode layer; preferably, the evaporation is thermal evaporation, and the evaporation rate is Preferably, the material of the second electrode layer includes at least one of gold, silver, copper, aluminum, and conductive oxide; preferably, the thickness of the second electrode layer is 80-200 nm.

[0012] In a second aspect, an embodiment of the present application provides a method for preparing a flexible solar cell module, comprising: providing a substrate; preparing a first oxide layer, a metal layer, and a second oxide layer in sequence on one side of the substrate, wherein the first oxide layer, the metal layer, and the second oxide layer constitute a first electrode layer; preparing a first transmission layer on a side of the first electrode layer away from the substrate; forming a perovskite active layer by single-source evaporation on a side of the first transmission layer away from the substrate; preparing a second transmission layer on a side of the perovskite active layer away from the substrate; and preparing a second electrode layer on a side of the second transmission layer away from the substrate.

[0013] In combination with the second aspect, a perovskite active layer is formed on a side of the first transport layer away from the substrate by single-source evaporation, comprising: using a single evaporation source, sequentially evaporating at least two layers of perovskite raw material layers on a surface of the first transport layer away from the substrate, and then performing annealing to obtain the perovskite active layer; preferably, the evaporation is thermal evaporation, and the evaporation rate is Preferably, the annealing temperature is 100-300° C., and the annealing time is 2-20 min; preferably, the raw materials of the perovskite include at least one of cesium iodide, methylamine iodide, and formamidine iodide, and lead iodide; preferably, the thickness of each layer of the perovskite raw material layer is 0.5 nm-30 nm, and the thickness of the perovskite active layer is 200-800 nm.

[0014] In a third aspect, an embodiment of the present application provides a method for preparing a flexible solar cell module, comprising: providing a substrate; preparing a first oxide layer by evaporation, preparing a metal layer by magnetron sputtering, and preparing a second oxide layer by evaporation on one side of the substrate, wherein the first oxide layer, the metal layer, and the second oxide layer constitute a first electrode layer; preparing a first transmission layer by magnetron sputtering on a side of the first electrode layer away from the substrate; preparing a perovskite active layer by evaporation on a side of the first transmission layer away from the substrate; preparing a second transmission layer by evaporation on a side of the perovskite active layer away from the substrate; and preparing a second electrode layer by evaporation on a side of the second transmission layer away from the substrate.

[0015] In a fourth aspect, an embodiment of the present application provides a flexible solar cell assembly, comprising: a substrate; a first electrode layer, disposed on one side of the substrate, the first electrode layer comprising a first oxide layer, a metal layer, and a second oxide layer stacked in sequence in a direction gradually away from the substrate; a first transmission layer, disposed on a side of the first electrode layer away from the substrate; a perovskite active layer, disposed on a side of the first transmission layer away from the substrate; a second transmission layer, disposed on a side of the perovskite active layer away from the substrate; and a second electrode layer, disposed on a side of the second transmission layer away from the substrate.

[0016] In combination with the fourth aspect, the material of the metal layer includes silver, and the thickness of the metal layer is 1 to 12 nm; preferably, the surface roughness of the first electrode layer is 5 to 30 nm; preferably, the surface resistance of the first electrode layer is 5 to 40 Ω / sq; preferably, the transmittance of the first electrode layer is 70% to 90%; preferably, the material of the first oxide layer and / or the material of the second oxide layer includes at least one of zinc oxide, tungsten oxide, and molybdenum oxide; preferably, the thickness of the first oxide layer and / or the thickness of the second oxide layer is 5 to 50 nm.

[0017] In a fifth aspect, an embodiment of the present application provides a flexible solar cell, which includes the above-mentioned flexible solar cell assembly, or the flexible solar cell includes a flexible solar cell assembly prepared according to the above-mentioned method.

[0018] Through the above technical scheme, in a mixture of argon and nitrogen, a metal layer is prepared by magnetron sputtering, which can increase the wettability of the metal layer on the first oxide layer, and obtain a first electrode layer with thin thickness, good density, low surface roughness and low surface resistance, thereby taking into account both light transmittance and conductivity, which is beneficial to improving the power conversion efficiency of perovskite solar cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic flow chart of a method for preparing a flexible solar cell module provided by an exemplary embodiment of the present application.

[0020] Figure 2 It is a schematic diagram of a method for preparing a flexible solar cell module provided by an exemplary embodiment of the present application.

[0021] Figure 3 It is a schematic flow chart of a method for preparing a flexible solar cell module provided by another exemplary embodiment of the present application.

[0022] Figure 4 It is a schematic flow chart of a method for preparing a flexible solar cell module provided by another exemplary embodiment of the present application.

[0023] Figure 5It is a schematic structural diagram of a flexible solar cell assembly provided by an exemplary embodiment of the present application. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0025] Perovskite has the characteristics of large absorption coefficient, long diffusion length, high mobility, and adjustable band gap. Due to its excellent performance, it has ushered in a new era of solar cell research. Up to now, the power conversion efficiency (PCE) of perovskite solar cells (PSCs) has exceeded 26%.

[0026] With the increasing demand for flexible solar cells, flexible solar cells have gradually become one of the research hotspots. Flexible perovskite solar cells have the characteristics of light weight and bendability, and can be applied to photovoltaic building integration, wearable devices, etc. However, at present, the research on perovskite solar cells mainly focuses on rigid solar cells, and flexible perovskite solar cells still face preparation difficulties.

[0027] First, as an optically active layer, perovskite should minimize defects during the preparation process to prevent defects from accumulating at the grain boundaries after repeated bending, thereby reducing the long-term stability of the device. Perovskite is extremely sensitive to water and oxygen, and can react with water and oxygen at room temperature to cause irreversible degradation. Therefore, in the entire preparation process, shielding the influence of water and oxygen and reducing perovskite defects caused by grain boundary erosion are crucial for the long-term stable operation of flexible PSCs.

[0028] Secondly, the transparent electrode currently used in flexible PSCs is indium tin oxide (ITO), but ITO is very brittle and will break after multiple bends, which greatly reduces the luminous efficiency and service life of flexible PSCs. In addition, ITO requires the use of rare element indium, which increases the preparation cost of the battery. Oxide / metal / oxide (OMO) electrodes are highly promising flexible electrodes, in which the metal material is mainly silver (Ag). When preparing the metal layer, silver grows in an island-like pattern, and a thicker metal layer needs to be coated to make the surface resistance of the OMO electrode lower; however, the thick metal layer will reduce the optical transmittance, resulting in a lower power conversion efficiency (PCE) of PSCs.

[0029] In view of the above problems, in a first aspect, an embodiment of the present application provides a method for preparing a flexible solar cell module.

[0030] Figure 1 It is a schematic flow chart of a method for preparing a flexible solar cell module provided by an exemplary embodiment of the present application. Figure 2 Schematic diagram of a method for preparing a flexible solar cell module provided by an exemplary embodiment of the present application. Figure 1 and Figure 2 The content shown is an exemplary introduction to the method for preparing the flexible solar cell module provided in the embodiment of the present application. Figure 1 As shown, the method includes the following steps.

[0031] Step S110, providing a substrate.

[0032] In the embodiment of the present application, the substrate is a flexible substrate. Figure 2 As shown, the material of the substrate 101 is polyimide (PI) or polyethylene terephthalate (PET). The size of the substrate is 1 to 10 cm, for example, the size of the substrate can be 1 cm, 3 cm, 5 cm, 8 cm, or 10 cm.

[0033] Before using the substrate to prepare perovskite solar cells, the substrate needs to be pretreated. For example, the substrate is ultrasonically cleaned using a first solvent, a second solvent, and a third solvent, and then dried. Optionally, the first solvent is acetone, the second solvent is ethanol, and the third solvent is deionized water. Use the first solvent to clean for 20 to 30 minutes (for example, 20 minutes, 30 minutes, 40 minutes), use the second solvent to ultrasonically clean for 20 to 40 minutes (for example, 20 minutes, 30 minutes, 40 minutes), and use the third solvent to ultrasonically clean for 20 to 40 minutes (for example, 20 minutes, 30 minutes, 40 minutes). The temperature of the drying treatment is 50 to 140°C (for example, 40°C, 60°C, 90°C, 100°C, 120°C, 140°C), and the time is 2 to 6 hours (for example, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours).

[0034] Step S120, a first oxide layer is formed on one side of the substrate, a metal layer is formed on the side of the first oxide layer away from the substrate by magnetron sputtering in a mixture of argon and nitrogen, and a second oxide layer is formed on the side of the metal layer away from the substrate. The first oxide layer, the metal layer and the second oxide layer constitute a first electrode layer.

[0035] In the embodiment of the present application, the first oxide layer is prepared on one side of the substrate, including: evaporating the material of the first oxide layer on one surface of the substrate 101 under vacuum to obtain the first oxide layer 1021, such as Figure 2 As shown. The evaporation is electron beam evaporation. The vacuum degree is 10 -3 ~10 -4 Pa, the evaporation rate is For example, the vacuum degree is 10 -4 Pa, 3*10 -4 Pa, 5*10 -4 Pa, 10 -3 Pa. The evaporation rate is The material of the first oxide layer 1021 includes at least one of zinc oxide (ZnO), oxide (WO3), and molybdenum oxide (MoO3). The thickness of the first oxide layer 1021 is 5 to 50 nm. Exemplarily, the thickness of the first oxide layer 1021 is 5 nm, 15 nm, 25 nm, 30 nm, 40 nm, 50 nm, etc.

[0036] In the embodiment of the present application, in a mixture of argon and nitrogen, a material of a metal layer is sputtered on a surface of the first oxide layer 1021 away from the substrate 101 to obtain a metal layer 1022, such as Figure 2 As shown. The gas pressure of the mixture of argon and nitrogen is 1 to 8 mTorr, the volume proportion of nitrogen in the mixture of argon and nitrogen is 0.01% to 1%, and the sputtering power is 100 to 500 W. Exemplarily, the gas pressure of the mixture of argon and nitrogen is 1 mTorr, 2 mTorr, 3 mTorr, 4 mTorr, 5 mTorr, 6 mTorr, 7 mTorr, and 8 mTorr. The volume proportion of nitrogen in the mixture of argon and nitrogen is 0.01%, 0.05%, 0.1%, 0.3%, 0.5%, 0.8%, and 1%. The sputtering power is 100 W, 150 W, 200 W, 300 W, 450 W, and 500 W. In an embodiment of the present application, the deposition rate of the metal layer is Exemplarily, the deposition rate of the metal layer is Optionally, the material of the metal layer 1022 is silver (Ag). Optionally, the thickness of the metal layer 1022 is 1-12 nm. Exemplarily, the thickness of the metal layer 1022 is 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 12 nm.

[0037] In the embodiment of the present application, a second oxide material is evaporated on the surface of the metal layer 1022 away from the substrate 101 under vacuum to obtain a second oxide layer 1023, such as Figure 2 As shown. The evaporation is electron beam evaporation. The vacuum degree is 10 -3~10 -4 Pa, the evaporation rate is For example, the vacuum degree is 10 -4 Pa, 3*10 -4 Pa, 5*10 -3 Pa, 10 -3 Pa. The evaporation rate is The material of the second oxide layer 1023 includes at least one of zinc oxide (ZnO), oxide (WO3), and molybdenum oxide (MoO3). The thickness of the second oxide layer 1023 is 5 to 50 nm. Exemplarily, the thickness of the second oxide layer 1023 is 5 nm, 15 nm, 25 nm, 30 nm, 40 nm, 50 nm, etc.

[0038] Optionally, the first oxide layer 1021 and the second oxide layer 1023 are made of the same material, and the first oxide layer 1021 and the second oxide layer 1023 are the same in thickness.

[0039] In the embodiment of the present application, the surface roughness of the first electrode layer 102 is 5-30 nm, the surface resistance of the first electrode layer 102 is 5-40 Ω / sq, and the transmittance of the first electrode layer 102 is 70%-90%.

[0040] The first oxide layer 1021, the metal layer 1022 and the second oxide layer 1023 constitute the first electrode layer 102. In the embodiment of the present application, the film layers of the first electrode layer 102 are prepared by combining electron beam evaporation and magnetron sputtering, which reduces the preparation time and has good quality of each prepared film layer. In addition, by preparing the metal layer 1022 by magnetron sputtering in a mixture of argon and nitrogen, the wettability of the metal layer (silver) 1022 on the first oxide layer 1021 can be increased, and the continuous growth of the metal layer 1022 can be achieved, thereby obtaining a first electrode layer 102 with a thinner thickness, better density, lower surface roughness and lower surface resistance, thereby taking into account both light transmittance and conductivity, which is beneficial to improving the power conversion efficiency of perovskite solar cells.

[0041] Step S130, preparing a first transmission layer on a side of the first electrode layer away from the substrate.

[0042] In the embodiment of the present application, in a mixture of argon and oxygen, the material of the first transmission layer is sputtered on the surface of the first electrode layer 102 away from the substrate 101 to obtain the first transmission layer 103, such as Figure 2As shown. The gas pressure of the mixture of argon and oxygen is 1 to 8 mTorr, the volume proportion of oxygen in the mixture of argon and oxygen is 0.01% to 2%, and the sputtering power is 100 to 500 W. Exemplarily, the gas pressure of the mixture of argon and oxygen is 1 mTorr, 2 mTorr, 3 mTorr, 4 mTorr, 5 mTorr, 6 mTorr, 7 mTorr, and 8 mTorr. The volume proportion of oxygen in the mixture of argon and oxygen is 0.01%, 0.05%, 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.3%, 1.5%, and 2%. The sputtering power is 100 W, 150 W, 200 W, 300 W, 450 W, and 500 W. In an embodiment of the present application, the deposition rate of the first transport layer 103 is Exemplarily, the deposition rate of the first transport layer 103 is In the embodiment of the present application, the material of the first transmission layer 103 is nickel oxide. The thickness of the first transmission layer 103 is 5-40 nm. Exemplarily, the thickness of the first transmission layer 103 is 5 nm, 10 nm, 15 nm, 25 nm, 30 nm, or 40 nm.

[0043] Step S140, preparing a perovskite active layer on a side of the first transmission layer away from the substrate.

[0044] In the embodiment of the present application, the perovskite active layer includes at least two layers of perovskite raw material layers. At least two layers of perovskite raw material layers are sequentially evaporated on the surface of the first transmission layer 103 away from the substrate 101, and then annealed to obtain the perovskite active layer 104, such as Figure 2 As shown. In an embodiment of the present application, the raw material layer of each layer of perovskite is prepared by single-source evaporation. The thickness of each layer of perovskite raw material layer is 0.5nm to 30nm. The thickness of the perovskite active layer is 200 to 800nm. Exemplarily, the thickness of the perovskite active layer is 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, and 800nm. The raw materials of perovskite include at least one of cesium iodide (CsI), methylamine iodide (MAI), formamidine iodide (FAI) and lead iodide (PbI2). In an embodiment of the present application, evaporation is thermal evaporation, and the evaporation rate is The annealing temperature is 100-300°C, and the annealing time is 2-20 minutes. Optionally, the evaporation rate is The annealing temperatures are 100°C, 120°C, 150°C, 200°C, 250°C, and 300°C. The annealing times are 2 min, 4 min, 8 min, 12 min, 16 min, and 20 min.

[0045] For example, the raw materials of the perovskite include lead iodide, cesium iodide, methylamine iodide and formamidine iodide. When preparing the perovskite active layer 104, the substrate coated with the first transmission layer 103 is moved into a thermal evaporation device, and a single-source evaporation is used to control the evaporation rate to Lead iodide, cesium iodide, methylamine iodide and formamidine iodide are sequentially evaporated, the thickness of each layer of the raw material layer of perovskite is 0.5nm to 30nm, and a total of 2 to 10 groups are evaporated. The thickness of the film layer after evaporation is 200 to 800nm, and then annealed at 100 to 300°C for 2 to 20min to obtain the perovskite active layer 104. By controlling the evaporation thickness of each layer of the raw material layer of the perovskite, the proportion and composition of each raw material in the perovskite active layer are regulated, and there is no need to accurately control the evaporation rate of different components, which reduces the requirements for equipment; and through multiple groups of evaporation, the raw materials of multiple perovskites are fully mixed to prepare a high-quality perovskite active layer 104. Optionally, according to the proportion and composition of each raw material in the perovskite active layer, the thickness of the raw material layers of different perovskites can be the same or different.

[0046] Step S150, preparing a second transmission layer on a side of the perovskite active layer away from the substrate.

[0047] In the embodiment of the present application, the material of the second transmission layer is evaporated on the surface of the perovskite active layer 104 away from the substrate 101 to obtain the second transmission layer 105, such as Figure 2 As shown. The evaporation is thermal evaporation, and the evaporation rate is Exemplarily, the evaporation rate is In an embodiment of the present application, the material of the second transmission layer 105 includes at least two of fullerene (C60), fullerene derivatives, phenyl C61 butyrate methyl ester (PCBM), and 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP). Exemplarily, the material of the second transmission layer 105 includes fullerene and BCP. The thickness of the second transmission layer 105 is 10 to 60 nm. Exemplarily, the thickness of the second transmission layer 105 is 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, and 60 nm.

[0048] Step S160, preparing a second electrode layer on a side of the second transmission layer away from the substrate.

[0049] In the embodiment of the present application, the material of the second electrode layer is evaporated on the surface of the second transmission layer 105 away from the substrate 101 to obtain the second electrode layer 106, such as Figure 2 As shown. The evaporation is thermal evaporation. The evaporation rate is Exemplarily, the evaporation rate is The material of the second electrode layer 106 includes a metal material, such as gold, silver, copper, aluminum, etc.; or the material of the second electrode layer 106 includes a conductive oxide, such as ITO, etc. The thickness of the second electrode layer 106 is 80 to 200 nm. Exemplarily, the thickness of the second electrode layer 106 is 80 nm, 100 nm, 120 nm, 150 nm, 170 nm, 180 nm, 200 nm.

[0050] In the embodiment of the present application, oxide / metal / oxide is used as the first electrode layer, so that the first electrode layer has good flexibility, and when applied to solar cells, it still has good power conversion efficiency after multiple bends. In addition, in a mixture of argon and nitrogen, the metal layer is prepared by magnetron sputtering, which can increase the wettability of the metal layer on the first oxide layer, thereby obtaining a first electrode layer with a thinner thickness, better density, lower surface roughness, and lower surface resistance, thereby taking into account both light transmittance and conductivity, which is beneficial to improving the power conversion efficiency of perovskite solar cells.

[0051] In a second aspect, an embodiment of the present application also provides a method for preparing a flexible solar cell module.

[0052] Figure 3 FIG. 1 is a flow chart of a method for preparing a flexible solar cell module provided by an exemplary embodiment of the present application. Figure 3 As shown, the method includes the following steps.

[0053] Step S310, providing a substrate.

[0054] Step S320: sequentially prepare a first oxide layer, a metal layer, and a second oxide layer on one side of the substrate. The first oxide layer, the metal layer, and the second oxide layer constitute a first electrode layer.

[0055] Step S330: preparing a first transmission layer on a side of the first electrode layer away from the substrate.

[0056] Step S340: forming a perovskite active layer on a side of the first transmission layer away from the substrate by single-source evaporation.

[0057] Using a single evaporation source, at least two layers of perovskite raw material layers are sequentially evaporated on the surface of the first transport layer away from the substrate, and then annealed to obtain a perovskite active layer. The thickness of each layer of perovskite raw material layer is 0.5nm to 30nm, and the thickness of the perovskite active layer is 200 to 800nm. Exemplarily, the thickness of the perovskite active layer is 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, and 800nm. The raw materials of perovskite include at least one of cesium iodide, methylamine iodide, and formamidine iodide and lead iodide. In an embodiment of the present application, the evaporation is thermal evaporation, and the evaporation rate is The annealing temperature is 100-300°C, and the annealing time is 2-20 minutes. Optionally, the evaporation rate is The annealing temperatures are 100°C, 120°C, 150°C, 200°C, 250°C, and 300°C. The annealing times are 2 min, 4 min, 8 min, 12 min, 16 min, and 20 min.

[0058] For example, the raw materials of the perovskite include lead iodide, cesium iodide, methylamine iodide and formamidine iodide. When preparing the perovskite active layer 104, the substrate coated with the first transmission layer 103 is moved into a thermal evaporation device, and a single-source evaporation is used to control the evaporation rate to Lead iodide, cesium iodide, methylamine iodide and formamidine iodide are sequentially evaporated, the thickness of each layer of the raw material layer of perovskite is 0.5nm to 30nm, and a total of 2 to 10 groups are evaporated. The thickness of the film layer after evaporation is 200 to 800nm, and then annealed at 100 to 300°C for 2 to 20min to obtain the perovskite active layer 104. By controlling the evaporation thickness of each layer of the raw material layer of the perovskite, the proportion and composition of each raw material in the perovskite active layer are regulated, and there is no need to accurately control the evaporation rate of different components, which reduces the requirements for equipment; and through multiple groups of evaporation, the raw materials of multiple perovskites are fully mixed to prepare a high-quality perovskite active layer 104. Optionally, according to the proportion and composition of each raw material in the perovskite active layer, the thickness of the raw material layers of different perovskites can be the same or different.

[0059] Step S350 , preparing a second transmission layer on a side of the perovskite active layer away from the substrate.

[0060] Step S360: preparing a second electrode layer on a side of the second transmission layer away from the substrate.

[0061] The preparation methods of steps S310 to S330 and steps S350 to S360 in the embodiment of the present application are the same as the preparation methods of steps S110 to S130 and steps S150 to S160, and are not described again here.

[0062] In an embodiment of the present application, single-source evaporation is utilized to sequentially evaporate at least two perovskite raw material layers on the surface of the first transport layer away from the substrate. By controlling the evaporation thickness of each perovskite raw material layer, the proportion and composition of each raw material in the perovskite active layer are regulated. There is no need to precisely control the evaporation rates of different components, thereby reducing the requirements for equipment. Furthermore, through multiple groups of evaporation, the raw materials of multiple perovskites are fully mixed to prepare a high-quality perovskite active layer.

[0063] In a third aspect, an embodiment of the present application also provides a method for preparing a flexible solar cell module.

[0064] Figure 4FIG. 1 is a flow chart of a method for preparing a flexible solar cell module provided by an exemplary embodiment of the present application. Figure 4 As shown, the method includes the following steps.

[0065] Step S410, providing a substrate.

[0066] Step S420, on one side of the substrate, a first oxide layer is formed by evaporation, a metal layer is formed by magnetron sputtering, and a second oxide layer is formed by evaporation. The first oxide layer, the metal layer and the second oxide layer constitute a first electrode layer.

[0067] Step S430: preparing a first transmission layer by magnetron sputtering on a side of the first electrode layer away from the substrate.

[0068] Step S440, preparing a perovskite active layer by evaporation on a side of the first transmission layer away from the substrate.

[0069] Step S450, preparing a second transmission layer by evaporation on a side of the perovskite active layer away from the substrate.

[0070] Step S460: Form a second electrode layer by evaporation on a side of the second transmission layer away from the substrate.

[0071] The specific contents of the preparation method in steps S410 to S460 in the embodiment of the present application are the same as those of the preparation method in steps S110 to S160, and will not be repeated here.

[0072] In the embodiments of the present application, when preparing each film layer of the perovskite solar cell, an evaporation or magnetron sputtering process is adopted, and no solution is used in the preparation process, thereby avoiding exposure of the perovskite active material to a water and oxygen environment during the preparation process, which may lead to a decrease in device function.

[0073] The above technical solution of the present application is described in detail below in conjunction with specific embodiments.

[0074] Example 1

[0075] The perovskite solar cell module prepared in this embodiment 1 includes the following steps:

[0076] Step 1: Treat the substrate. Use acetone to ultrasonically clean the polyimide substrate for 30 minutes, then use ethanol to ultrasonically clean the polyimide substrate for 30 minutes, and finally use deionized water to ultrasonically clean the polyimide substrate for 30 minutes. Then put the cleaned polyimide substrate into an oven and bake it at 100°C for 5 hours.

[0077] Step 2: Prepare the first electrode layer. Place the treated substrate into the electron beam evaporation chamber and evacuate to 10 -4 Pa, the evaporation rate is Zinc oxide was evaporated to a thickness of 15 nm. Then the substrate was moved into the magnetron sputtering equipment, argon and nitrogen were injected, the volume proportion of nitrogen was controlled to be 0.1%, the pressure was 2 mTorr, the power was 200 W, and silver was sputtered at a deposition rate of The thickness of the sputtered silver is 3nm. The substrate coated with the metal layer is placed in the electron beam evaporation chamber again and evacuated to 10 -4 Pa, the evaporation rate is Zinc oxide was evaporated to a thickness of 15 nm to obtain a flexible first electrode layer.

[0078] Step 3: Prepare the first transmission layer. Move the substrate coated with the first electrode layer into the magnetron sputtering equipment, inject argon and oxygen, control the volume proportion of oxygen to 0.1%, the pressure to 4mTorr, the power to 150W, and sputter nickel oxide. The deposition rate of nickel oxide is The thickness of the sputtered nickel oxide was 30 nm.

[0079] Step 4: Prepare the perovskite active layer. Move the substrate coated with the first transmission layer into the thermal evaporation equipment, use single-source evaporation, and control the evaporation rate to Lead iodide, cesium iodide, methylamine iodide and formamidine iodide were sequentially deposited, the thickness of each perovskite raw material layer was 20nm, a total of 5 groups were deposited, the film thickness after the deposition was 400nm, and annealed at 100℃ for 20min to obtain the perovskite active layer. The thickness of the perovskite active layer is 400nm.

[0080] Step 5: Prepare the second transport layer. On the substrate coated with the perovskite active layer, C60 and BCP are sequentially evaporated at a rate of The second transmission layer is obtained. The thickness of the second transmission layer is 30 nm.

[0081] Step 6: Prepare the second electrode layer. On the substrate coated with the second transmission layer, evaporate silver at a rate of The second electrode layer is obtained. The thickness of the second electrode layer is 120 nm.

[0082] Example 2

[0083] The perovskite solar cell prepared in this embodiment 2 includes the following steps:

[0084] Step 1: Treat the substrate. Use acetone to ultrasonically clean the polyimide substrate for 30 minutes, then use ethanol to ultrasonically clean the polyimide substrate for 30 minutes, and finally use deionized water to ultrasonically clean the polyimide substrate for 30 minutes. Then put the cleaned polyimide substrate into an oven and bake it at 100°C for 5 hours.

[0085] Step 2: Prepare the first electrode layer. Place the treated substrate into the electron beam evaporation chamber and evacuate to 10 -4 Pa, the evaporation rate is Zinc oxide was evaporated to a thickness of 15 nm. Then the substrate was moved into the magnetron sputtering equipment, argon and nitrogen were injected, the volume proportion of nitrogen was controlled to be 0.1%, the pressure was 2 mTorr, the power was 200 W, and silver was sputtered at a deposition rate of The thickness of the sputtered silver is 6nm. The substrate coated with the metal layer is placed in the electron beam evaporation chamber again and evacuated to 10 -4 Pa, the evaporation rate is Zinc oxide was evaporated to a thickness of 15 nm to obtain a flexible first electrode layer.

[0086] Step 3: Prepare the first transmission layer. Move the substrate coated with the first electrode layer into the magnetron sputtering equipment, inject argon and oxygen, control the volume proportion of oxygen to 0.1%, the pressure to 4mTorr, the power to 150W, and sputter nickel oxide. The deposition rate of nickel oxide is The thickness of the sputtered nickel oxide was 30 nm.

[0087] Step 4: Prepare the perovskite active layer. The substrate coated with the first transmission layer is introduced into the thermal evaporation equipment, and single-source evaporation is used to control the evaporation rate to Lead iodide, cesium iodide, methylamine iodide and formamidine iodide were sequentially deposited, the thickness of each perovskite raw material layer was 20nm, a total of 5 groups were deposited, the film thickness after the deposition was 400nm, and annealed at 100℃ for 20min to obtain the perovskite active layer. The thickness of the perovskite active layer is 400nm.

[0088] Step 5: Prepare the second transport layer. On the substrate coated with the perovskite active layer, C60 and BCP are sequentially evaporated at a rate of The second transmission layer is obtained. The thickness of the second transmission layer is 30 nm.

[0089] Step 6: Prepare the second electrode layer. On the substrate coated with the second transmission layer, evaporate silver at a rate of The second electrode layer is obtained. The thickness of the second electrode layer is 120 nm.

[0090] Example 3

[0091] The perovskite solar cell module prepared in this embodiment 3 includes the following steps:

[0092] Step 1: Treat the substrate. Use acetone to ultrasonically clean the polyimide substrate for 30 minutes, then use ethanol to ultrasonically clean the polyimide substrate for 30 minutes, and finally use deionized water to ultrasonically clean the polyimide substrate for 30 minutes. Then put the cleaned polyimide substrate into an oven and bake it at 100°C for 5 hours.

[0093] Step 2: Prepare the first electrode layer. Place the treated substrate into the electron beam evaporation chamber and evacuate to 10 -4 Pa, the evaporation rate is Zinc oxide was evaporated to a thickness of 15 nm. Then the substrate was moved into the magnetron sputtering equipment, argon and nitrogen were injected, the volume proportion of nitrogen was controlled to be 0.1%, the pressure was 2 mTorr, the power was 200 W, and silver was sputtered at a deposition rate of The thickness of the sputtered silver is 9 nm. The substrate coated with the metal layer is placed in the electron beam evaporation chamber again and evacuated to 10 -4 Pa, the evaporation rate is Zinc oxide was evaporated to a thickness of 15 nm to obtain a flexible first electrode layer.

[0094] Step 3: Prepare the first transmission layer. Move the substrate coated with the first electrode layer into the magnetron sputtering equipment, inject argon and oxygen, control the volume proportion of oxygen to 0.1%, the pressure to 4mTorr, the power to 150W, and sputter nickel oxide. The deposition rate of nickel oxide is The thickness of the sputtered nickel oxide was 30 nm.

[0095] Step 4: Prepare the perovskite active layer. The substrate coated with the first transmission layer is introduced into the thermal evaporation equipment, and single-source evaporation is used to control the evaporation rate to Lead iodide, cesium iodide, methylamine iodide and formamidine iodide were sequentially deposited, the thickness of each perovskite raw material layer was 20nm, a total of 5 groups were deposited, the film thickness after the deposition was 400nm, and annealed at 100℃ for 20min to obtain the perovskite active layer. The thickness of the perovskite active layer is 400nm.

[0096] Step 5: Prepare the second transmission layer. On the substrate coated with the perovskite active layer, C60 and PCBM are sequentially evaporated at a rate of The second transmission layer is obtained. The thickness of the second transmission layer is 30 nm.

[0097] Step 6: Prepare the second electrode layer. On the substrate coated with the second transmission layer, evaporate silver at a rate of The second electrode layer is obtained. The thickness of the second electrode layer is 120 nm.

[0098] Example 4

[0099] The perovskite solar cell module prepared in this embodiment 4 includes the following steps:

[0100] Step 1: Treat the substrate. Use acetone to ultrasonically clean the polyimide substrate for 30 minutes, then use ethanol to ultrasonically clean the polyimide substrate for 30 minutes, and finally use deionized water to ultrasonically clean the polyimide substrate for 30 minutes. Then put the cleaned polyimide substrate into an oven and bake it at 100°C for 5 hours.

[0101] Step 2: Prepare the first electrode layer. Place the treated substrate into the electron beam evaporation chamber and evacuate to 10 -4 Pa, the evaporation rate is Zinc oxide was evaporated to a thickness of 15 nm. Then the substrate was moved into the magnetron sputtering equipment, argon and nitrogen were injected, the volume proportion of nitrogen was controlled to be 0.1%, the pressure was 2 mTorr, the power was 200 W, and silver was sputtered at a deposition rate of The thickness of the sputtered silver is 12nm. The substrate coated with the metal layer is placed in the electron beam evaporation chamber again and evacuated to 10 -4 Pa, the evaporation rate is Zinc oxide was evaporated to a thickness of 15 nm to obtain a flexible first electrode layer.

[0102] Step 3: Prepare the first transmission layer. Move the substrate coated with the first electrode layer into the magnetron sputtering equipment, inject argon and oxygen, control the volume proportion of oxygen to 0.1%, the pressure to 4mTorr, the power to 150W, and sputter nickel oxide. The deposition rate of nickel oxide is The thickness of the sputtered nickel oxide was 30 nm.

[0103] Step 4: Prepare the perovskite active layer. The substrate coated with the first transmission layer is introduced into the thermal evaporation equipment, and single-source evaporation is used to control the evaporation rate to Lead iodide, cesium iodide, methylamine iodide and formamidine iodide were sequentially deposited, the thickness of each perovskite raw material layer was 20nm, a total of 5 groups were deposited, the film thickness after the deposition was 400nm, and annealed at 100℃ for 20min to obtain the perovskite active layer. The thickness of the perovskite active layer is 400nm.

[0104] Step 5: Prepare the second transport layer. On the substrate coated with the perovskite active layer, C60 and BCP are sequentially evaporated at a rate of The second transmission layer is obtained. The thickness of the second transmission layer is 30 nm.

[0105] Step 6: Prepare the second electrode layer. On the substrate coated with the second transmission layer, evaporate silver at a rate of The second electrode layer is obtained. The thickness of the second electrode layer is 120 nm.

[0106] Comparative Example 1

[0107] The difference between Comparative Example 1 and Example 1 is: the step of preparing the metal layer in step 2. In Comparative Example 1, metallic silver is sputtered in pure argon gas, and the thickness of the sputtered silver is 3 nm.

[0108] Comparative Example 2

[0109] The difference between Comparative Example 2 and Example 2 is: the step of preparing the metal layer in step 2. In Comparative Example 1, metallic silver is sputtered in pure argon gas, and the thickness of the sputtered silver is 6 nm.

[0110] Comparative Example 3

[0111] The difference between Comparative Example 3 and Example 3 is: the step of preparing the metal layer in step 2. In Comparative Example 1, metallic silver is sputtered in pure argon gas, and the thickness of the sputtered silver is 9 nm.

[0112] Comparative Example 4

[0113] The difference between Comparative Example 4 and Example 4 is: the step of preparing the metal layer in step 2. In Comparative Example 1, metallic silver is sputtered in pure argon gas, and the thickness of the sputtered silver is 12 nm.

[0114] Comparative Example 5

[0115] The difference between Comparative Example 5 and Example 1 is that the material of the first electrode layer in step 2 is ITO, and the thickness is 150 nm.

[0116] The following is an analysis in combination with Examples 1 to 4 and Comparative Examples 1 to 5.

[0117] Table 1 shows the surface resistance of the first electrode layer of Examples 1 to 4 and Comparative Examples 1 to 4.

[0118]

[0119] It can be seen from Table 1 that when the thickness of the metal layer Ag is the same, the surface resistance of the first electrode layer prepared in the mixture of argon and nitrogen is lower than that of the first electrode layer prepared in pure argon. This is because, in pure argon, silver has poor wettability on a heterogeneous matrix (e.g., the first oxide layer), and tends to grow in an island shape when sputtering silver, resulting in poor compactness of the metal layer and high surface resistance. In the mixture of argon and nitrogen, nitrogen can enhance the wettability of metallic silver on the first oxide layer, and silver can grow continuously. The first electrode layer finally prepared has good compactness, low surface roughness, low surface resistance, and good light transmittance. In addition, the volume proportion of nitrogen in the mixed gas is controlled at 0.01% to 1%. If the nitrogen content is too high, it will affect the growth mode of silver, thereby increasing the surface resistance of the first electrode layer.

[0120] Table 2 shows the power conversion efficiency (PCE) of the perovskite solar cells of Example 1 and Comparative Example 5.

[0121] Example PCE without bending PCE after 1000 bending cycles Example 1 16.5% 15.5% Comparative Example 5 14.1% 9.7%

[0122] It can be seen from Table 2 that when not bent, the PCE of the perovskite solar cell with OMO as the first electrode layer is slightly better than the PCE of the perovskite solar cell with ITO as the first electrode layer. After bending 1000 times, the PCE of the perovskite solar cell with OMO as the first electrode layer only decreased slightly; while the PCE of the perovskite solar cell with ITO as the first electrode layer decreased significantly. This is because the ITO electrode has great brittleness and will break after multiple bending, which greatly reduces the PCE of the perovskite solar cell and reduces the service life of the battery. The OMO electrode has good flexibility and is still not easy to break after multiple bending, allowing the battery to maintain good PCE performance.

[0123] In a fourth aspect, an embodiment of the present application provides a flexible solar cell module.

[0124] Figure 5 Schematic diagram of the structure of a flexible solar cell module provided by an exemplary embodiment of the present application. Figure 5 As shown, the flexible solar cell assembly includes a substrate 101, a first electrode layer 102, a first transmission layer 103, a perovskite active layer 104, a second transmission layer 105, and a second electrode layer 106. The first electrode layer 102 is disposed on one side of the substrate 101. The first transmission layer 103 is disposed on a side of the first electrode layer 102 away from the substrate 101. The perovskite active layer 104 is disposed on a side of the first transmission layer 103 away from the substrate 101. The second transmission layer 105 is disposed on a side of the perovskite active layer 104 away from the substrate 101. The second electrode layer 106 is disposed on a side of the second transmission layer 105 away from the substrate 101.

[0125] The first electrode layer 102 includes a first oxide layer 1021, a metal layer 1022, and a second oxide layer 1023 stacked in sequence in a direction gradually away from the substrate 101. The material of the metal layer 1022 includes silver, and the thickness of the metal layer 1022 is 1 to 12 nm. Exemplarily, the thickness of the metal layer 1022 is 1 nm, 3 nm, 4 nm, 6 nm, 8 nm, 9 nm, 10 nm, 12 nm. The material of the first oxide layer 1021 and / or the second oxide layer 1023 includes at least one of zinc oxide, tungsten oxide, and molybdenum oxide. The thickness of the first oxide layer 1021 and / or the thickness of the second oxide layer 1023 is 5 to 50 nm. Exemplarily, the thickness of the first oxide layer 1021 and / or the thickness of the second oxide layer 1023 is 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm.

[0126] In the embodiment of the present application, the surface roughness of the first electrode layer 102 is 5-30 nm, the surface resistance of the first electrode layer 102 is 5-40 Ω / sq, and the transmittance of the first electrode layer 102 is 70%-90%.

[0127] In the embodiment of the present application, oxide / metal / oxide is used as the first electrode layer, so that the first electrode layer has good flexibility, and when applied to a solar cell, it still has good power conversion efficiency after multiple bends. In addition, the first electrode layer in the embodiment of the present application has a thin thickness, good density, low surface roughness, and low surface resistance, which can take into account both transmittance and conductivity, and is conducive to improving the power conversion efficiency of the perovskite solar cell.

[0128] In a fifth aspect, an embodiment of the present application provides a flexible solar cell, which includes a flexible solar cell assembly prepared according to the above method.

[0129] The basic principles of the present application are described above in conjunction with specific embodiments. However, it should be noted that the advantages, strengths, effects, etc. mentioned in the present application are only examples and not limitations, and it cannot be considered that these advantages, strengths, effects, etc. are required by each embodiment of the present application. In addition, the specific details disclosed above are only for the purpose of illustration and ease of understanding, not for limitation, and the above details do not limit the present application to being implemented by adopting the above specific details.

[0130] The block diagrams of the devices, apparatuses, equipment, and systems involved in this application are only illustrative examples and are not intended to require or imply that they must be connected, arranged, and configured in the manner shown in the block diagram. As will be appreciated by those skilled in the art, these devices, apparatuses, equipment, and systems can be connected, arranged, and configured in any manner. Words such as "including", "comprising", "having", etc. are open words, referring to "including but not limited to", and can be used interchangeably with them. The words "or" and "and" used here refer to the words "and / or" and can be used interchangeably with them, unless the context clearly indicates otherwise. The words "such as" used here refer to the phrase "such as but not limited to", and can be used interchangeably with them.

[0131] It should also be noted that in the apparatus, device and method of the present application, each component or each step can be decomposed and / or recombined. Such decomposition and / or recombination should be regarded as equivalent solutions of the present application.

[0132] The above description of the disclosed aspects is provided to enable any person skilled in the art to make or use the present application. Various modifications to these aspects will be readily apparent to those skilled in the art, and the general principles defined herein may be applied to other aspects without departing from the scope of the present application. Therefore, the present application is not intended to be limited to the aspects shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

[0133] The above description has been given for the purpose of illustration and description. In addition, this description is not intended to limit the embodiments of the present application to the forms disclosed herein. Although multiple example aspects and embodiments have been discussed above, those skilled in the art will recognize certain variations, modifications, changes, additions and sub-combinations thereof.

Claims

1. A method for preparing a flexible solar cell module, characterized in that: include: providing a substrate; A first oxide layer is prepared on one side of the substrate, a metal layer is prepared by magnetron sputtering on a side of the first oxide layer away from the substrate in a mixed gas of argon and nitrogen, and a second oxide layer is prepared on a side of the metal layer away from the substrate, wherein the first oxide layer, the metal layer and the second oxide layer constitute a first electrode layer; Preparing a first transmission layer on a side of the first electrode layer away from the substrate; Preparing a perovskite active layer on a side of the first transmission layer away from the substrate; Preparing a second transmission layer on a side of the perovskite active layer away from the substrate; A second electrode layer is formed on a side of the second transmission layer away from the substrate.

2. The method according to claim 1, characterized in that: The method of preparing a metal layer by magnetron sputtering on a side of the first oxide layer away from the substrate in a mixed gas of argon and nitrogen comprises: The gas pressure of the mixed gas of argon and nitrogen is 1 to 8 mTorr, and the volume proportion of nitrogen in the mixed gas of argon and nitrogen is 0.01% to 1%. Preferably, the sputtering power is 100 to 500 W; Preferably, the deposition rate of the metal layer is Preferably, the material of the metal layer is silver; Preferably, the thickness of the metal layer is 1-12 nm.

3. The method according to claim 1, characterized in that The step of preparing a first oxide layer on one side of the substrate comprises: Under vacuum, evaporating the material of the first oxide layer on one surface of the substrate to obtain the first oxide layer; Preferably, the evaporation is electron beam evaporation; Preferably, the vacuum degree of the vacuum is 10 -3 ~10 -4 Pa, the evaporation rate is Preferably, the material of the first oxide layer includes at least one of zinc oxide, tungsten oxide and molybdenum oxide; Preferably, the thickness of the first oxide layer is 5-50 nm; and / or The step of preparing a second oxide layer on a side of the metal layer away from the substrate comprises: Under vacuum, evaporating the second oxide material on the surface of the metal layer away from the substrate to obtain the second oxide layer; Preferably, the evaporation is electron beam evaporation; Preferably, the vacuum degree of the vacuum is 10 -3 ~10 -4 Pa, the evaporation rate is Preferably, the material of the second oxide layer includes at least one of zinc oxide, tungsten oxide and molybdenum oxide; Preferably, the second oxide layer has a thickness of 5-50 nm.

4. The method according to any one of claims 1 to 3, characterized in that: The perovskite active layer includes at least two layers of perovskite raw material layers, and the step of preparing the perovskite active layer on a side of the first transmission layer away from the substrate includes: Sequentially evaporating the at least two layers of perovskite raw material layers on the surface of the first transmission layer away from the substrate, and then performing annealing treatment to obtain the perovskite active layer; Preferably, the evaporation is thermal evaporation, and the evaporation rate is Preferably, each layer of the raw material of the perovskite is prepared by single-source evaporation; Preferably, the annealing temperature is 100 to 300° C., and the annealing time is 2 to 20 min; Preferably, the raw materials of the perovskite include lead iodide and at least one of cesium iodide, methylamine iodide and formamidine iodide; Preferably, the thickness of each layer of the perovskite raw material layer is 0.5 nm to 30 nm, and the thickness of the perovskite active layer is 200 to 800 nm; Preferably, the step of preparing the first transmission layer on a side of the first electrode layer away from the substrate comprises: In a mixed gas of argon and oxygen, sputtering a material of the first transmission layer on a surface of the first electrode layer away from the substrate to obtain the first transmission layer; Preferably, the gas pressure of the mixed gas of argon and oxygen is 1 to 8 mTorr, and the volume proportion of oxygen in the mixed gas of argon and oxygen is 0.01% to 2%; Preferably, the sputtering power is 100 to 500 W; Preferably, the deposition rate of the first transport layer is Preferably, the material of the first transmission layer is nickel oxide; Preferably, the thickness of the first transmission layer is 5 to 40 nm; Preferably, the step of preparing a second transmission layer on a side of the perovskite active layer away from the substrate comprises: Vapor depositing the material of the second transmission layer on the surface of the perovskite active layer away from the substrate to obtain the second transmission layer; Preferably, the evaporation is thermal evaporation, and the evaporation rate is Preferably, the material of the second transmission layer includes at least two of fullerene, fullerene derivatives, phenyl C61 butyric acid methyl ester, and 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline; Preferably, the thickness of the second transmission layer is 10 to 60 nm; Preferably, the step of preparing a second electrode layer on a side of the second transmission layer away from the substrate comprises: Vapor depositing the material of the second electrode layer on the surface of the second transmission layer away from the substrate to obtain the second electrode layer; Preferably, the evaporation is thermal evaporation, and the evaporation rate is Preferably, the material of the second electrode layer includes at least one of gold, silver, copper, aluminum, and conductive oxide; Preferably, the thickness of the second electrode layer is 80-200 nm.

5. A method for preparing a flexible solar cell module, characterized in that: include: providing a substrate; Sequentially preparing a first oxide layer, a metal layer, and a second oxide layer on one side of the substrate, wherein the first oxide layer, the metal layer, and the second oxide layer constitute a first electrode layer; Preparing a first transmission layer on a side of the first electrode layer away from the substrate; On a side of the first transmission layer away from the substrate, forming a perovskite active layer by single-source evaporation; Preparing a second transmission layer on a side of the perovskite active layer away from the substrate; A second electrode layer is formed on a side of the second transmission layer away from the substrate.

6. The method according to claim 5, characterized in that The method of forming a perovskite active layer on a side of the first transmission layer away from the substrate by single-source evaporation comprises: Using a single evaporation source, sequentially evaporating at least two layers of perovskite raw material layers on the surface of the first transmission layer away from the substrate, and then performing annealing treatment to obtain the perovskite active layer; Preferably, the evaporation is thermal evaporation, and the evaporation rate is Preferably, the annealing temperature is 100 to 300° C., and the annealing time is 2 to 20 min; Preferably, the raw materials of the perovskite include at least one of cesium iodide, methylamine iodide, formamidine iodide and lead iodide; Preferably, the thickness of each layer of the perovskite raw material layer is 0.5 nm to 30 nm, and the thickness of the perovskite active layer is 200 to 800 nm.

7. A method for preparing a flexible solar cell module, characterized in that: include: providing a substrate; On one side of the substrate, a first oxide layer is sequentially formed by evaporation, a metal layer is formed by magnetron sputtering, and a second oxide layer is formed by evaporation, wherein the first oxide layer, the metal layer and the second oxide layer constitute a first electrode layer; Forming a first transmission layer on a side of the first electrode layer away from the substrate by magnetron sputtering; Preparing a perovskite active layer by evaporation on a side of the first transmission layer away from the substrate; Preparing a second transmission layer by evaporation on a side of the perovskite active layer away from the substrate; A second electrode layer is formed by evaporation on a side of the second transmission layer away from the substrate.

8. A flexible solar cell module, characterized in that: include: substrate; A first electrode layer is provided on one side of the substrate, the first electrode layer comprising a first oxide layer, a metal layer, and a second oxide layer stacked in sequence in a direction gradually away from the substrate; A first transmission layer, disposed on a side of the first electrode layer away from the substrate; A perovskite active layer, disposed on a side of the first transmission layer away from the substrate; A second transmission layer is disposed on a side of the perovskite active layer away from the substrate; The second electrode layer is arranged on a side of the second transmission layer away from the substrate.

9. The flexible solar cell assembly according to claim 8, characterized in that: The material of the metal layer includes silver, and the thickness of the metal layer is 1 to 12 nm; Preferably, the surface roughness of the first electrode layer is 5 to 30 nm; Preferably, the surface resistance of the first electrode layer is 5 to 40Ω / sq; Preferably, the transmittance of the first electrode layer is 70% to 90%; Preferably, the material of the first oxide layer and / or the material of the second oxide layer includes at least one of zinc oxide, tungsten oxide and molybdenum oxide; Preferably, the thickness of the first oxide layer and / or the thickness of the second oxide layer is 5-50 nm.

10. A flexible solar cell, characterized in that: The flexible solar cell comprises the flexible solar cell assembly according to claim 8 or 9, or the flexible solar cell comprises the flexible solar cell assembly prepared by the method according to any one of claims 1 to 7.