Method for operating blast furnace
By adjusting the alkalinity of the total raw material components of iron-based raw materials and sub-raw materials in the blast furnace, the composition of high-concentration reduction gas is ensured, and the problem of reducing ventilation caused by the reduction of FeO components in the blast furnace before the air outlet is solved, and stable ventilation in the blast furnace is achieved and slag dripping properties.
Patent Information
- Application Number
- CN202280094341.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-11
- Filing Date
- 2022-12-16
- Publication Date
- 2024-11-26
AI Technical Summary
When high concentration reduction gas is generated in the blast furnace in front of the air outlet, the prior art fails to effectively ensure that the reduction of FeO component in the slag does not lead to a reduction in ventilation properties and slag retention, resulting in increased ventilation resistance and gas bleeding.
By loading iron-based raw materials, secondary raw materials and coke on the top of the blast furnace, and blowing high-concentration reduction gas from the air outlet, adjusting the alkalinity of the total raw material components to the range of 1.0 or above and below 1.7 to ensure that the high-concentration reduction gas is from H2, N2 and CO are composed of a proportion within a specific area to improve the liquidity and aeration properties of the slag.
In the blast furnace operation in front of the air outlet, by adjusting the alkalinity of the total raw material components, the aerability of the soft melting belt and dripping belt in the blast furnace can be maintained, ensuring that the viscosity of the slag is within the operable range, and the stable operation of the blast furnace can be achieved.
Smart Images

Figure CN119032183A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for operating a blast furnace in which a high-concentration reducing gas is generated in the blast furnace before the tuyere, and more particularly to a method for operating a blast furnace in which the properties of slag in the soft melting zone and the dripping zone in the blast furnace are improved and the air permeability in the blast furnace is increased. Background Art
[0002] In recent years, there has been a growing trend to reduce the emission of CO2 gas (carbon dioxide gas), which is one of the greenhouse gases. In the ironmaking method using a blast furnace, a large amount of CO2 gas is generated because carbon materials are used as reducing materials. Therefore, the steel industry has become one of the main industries in terms of CO2 gas emissions and must meet social demands for reducing CO2 gas emissions. Specifically, it has become a top priority to further reduce the ratio of reducing materials from coal in blast furnace operations. The ratio of reducing materials from coal refers to the total mass of coke from coal and reducing gas from coal required to produce 1 ton of molten iron.
[0003] The reducing materials have the function of becoming heat in the furnace to raise the temperature of the charge and reducing the iron ore, sintered ore and granular ore which are the iron-based raw materials in the furnace. In order to reduce the reduction material ratio and reduce the emission of CO2 gas, it is necessary to improve the reduction efficiency of the reducing materials while maintaining the heat in the furnace.
[0004] As a reducing material for the purpose of reducing CO2 gas emissions, hydrogen has attracted attention. The reduction of iron ore using hydrogen is an endothermic reaction, but its endothermic heat is smaller than that of a direct reduction reaction (reaction formula: FeO+C→Fe+CO), and the reduction rate using hydrogen is faster than that using CO gas. Therefore, by blowing hydrogen-based gas into the blast furnace, it is possible to simultaneously reduce CO2 gas emissions and improve reduction efficiency.
[0005] For stable operation of a blast furnace, it is necessary to ensure the air permeability of the remelting zone where the iron-based raw materials are remelted in the blast furnace. However, in blast furnace operations where a high concentration of reducing gas is generated in the furnace before the tuyere and where the reducing gas concentration in the furnace is high and the reduction reaction rate is faster than in conventional operations, the air permeability in the blast furnace is still unclear.
[0006] Blast furnaces produce a large amount of blast furnace slag (oxides composed of FeO, CaO, Al2O3, MgO, SiO2, etc.) as a by-product while producing pig iron. In order to maintain good air permeability in the furnace, it is necessary to design raw materials that can suppress the viscosity of the produced blast furnace slag to a low level and ensure liquid permeability.
[0007] As conventional techniques for solving problems similar to the above-mentioned problems, techniques disclosed in Patent Documents 1 to 3 are proposed.
[0008] Patent Document 1 discloses a blast furnace operation in which coke is charged from the furnace top and auxiliary fuel is blown from the tuyere. According to Patent Document 1, by setting the ratio of Al2O3 to SiO2 (Al2O3 / SiO2) of coke and auxiliary fuel to 0.6 or more and the basicity of blast furnace slag ((CaO+Al2O3+MgO) / SiO2) to 1.8 or more, the properties of blast furnace slag can be improved, and the gas permeability and liquid permeability can be improved.
[0009] Patent Document 2 discloses a blast furnace operation method in which 150 kg or more of pulverized coal is blown into the blast furnace from the tuyere together with hot air for every ton of iron produced. According to Patent Document 2, by using sintered ore having a SiO2 component of 4.0 to 4.8 mass %, a MgO component of 1.2 to 2.4 mass %, a CaO component of 6.0 to 9.0 mass %, and an Al2O3 component of 1.9 to 2.5 mass % as more than 80% of the charge other than coke charged from the furnace top, the viscosity of the dripping slag can be suppressed to a low level even if the FeO component of the slag composition is reduced.
[0010] Patent Document 3 discloses a blast furnace operation method using a sintered ore with high strength (SI>92%) and high reducibility (RI>70%) by adjusting the ratio of auxiliary raw materials according to the amount of Al2O3 in the sintered ore commonly used. According to Patent Document 3, by blowing an auxiliary raw material in an amount corresponding to the difference in the ratio of auxiliary raw materials between the sintered ore with high strength and high reducibility and the sintered ore commonly used from the blast furnace tuyere, high ore / reduced material ratio operation can be performed stably for a long period of time.
[0011] Prior art literature
[0012] Patent Literature
[0013] Patent Document 1: Japanese Patent Application Publication No. 2004-10948
[0014] Patent Document 2: Japanese Patent Application Laid-Open No. 9-13107
[0015] Patent Document 3: Japanese Patent Application Publication No. 2005-298923 Summary of the invention
[0016] Problems to be solved by the invention
[0017] However, these prior arts all focus on blast furnace operations in which auxiliary raw materials such as SiO2 powder, auxiliary fuels containing CaO, SiO2, etc., or pulverized coal are blown into the blast furnace through the tuyere, and do not mention the charged raw material components and slag components in the blast furnace operation in which a high concentration of reducing gas is produced in the furnace in front of the tuyere.
[0018] In the blast furnace operation of the present invention, the concentration of the reducing gas generated in the furnace before the tuyere is very high. Therefore, the reduction rate of the iron-based raw materials increases and the FeO concentration in the slag decreases in the furnace, and the FeO content in the slag decreases to a range lower than the operating range described in the above-mentioned prior art. The above-mentioned prior art does not consider the situation where the FeO content in the slag is further reduced.
[0019] That is, in the high concentration reducing gas generated in the furnace before the tuyere Figure 1 ( Figure 1 In the case of operating in the range of region A (described later) (including H2 gas = 0 to 100 volume%, N2 gas = 0 to 71 volume%, CO gas = 0 to 100 volume%), the reduction of the iron-based raw materials from low temperature is promoted to a level higher than in the previous operation, so the reduction rate of the iron-based raw materials reaching the lower part of the furnace increases. In this case, under the state of the previous operation method, there is a concern that the slag permeability will decrease due to the reduction of the FeO component in the slag, the slag will be retained in the gaps of the coke layer, and the ventilation resistance in the furnace will increase, inducing gas blowby.
[0020] The present invention has been completed in view of the above situation, and its purpose is to provide a blast furnace operation method, which improves the slag properties when implementing blast furnace operation in which a high concentration of reducing gas is generated in the furnace before the tuyere, and even if the FeO component in the slag is reduced, the permeability in the soft melting zone and dripping zone in the blast furnace can be ensured.
[0021] Methods used to solve problems
[0022] The gist of the present invention for solving the above-mentioned problems is as follows.
[0023] [1] A method for operating a blast furnace, which comprises charging iron-based raw materials, auxiliary raw materials and coke from the top of the blast furnace and blowing gas from the tuyere of the blast furnace into the furnace in front of the tuyere to produce a high-concentration reducing gas, wherein the basicity of the total raw material component of the above-mentioned iron-based raw materials and the above-mentioned auxiliary raw materials is set within a specified range.
[0024] [2] The blast furnace operating method according to [1], wherein the basicity of the total raw material components is set within a range of 1.0 to 1.7.
[0025] [3] The operating method of a blast furnace according to [1], wherein, when expressed in terms of the bosh gas composition, the high-concentration reducing gas is composed of H2 gas, N2 gas and CO gas, and the ratio of H2 gas, N2 gas and CO gas is a composition within an area surrounded by four points in the ternary phase diagram of H2 gas-N2 gas-CO gas: H2 gas: 0 volume%, N2 gas: 0 volume%, CO gas: 100 volume%, H2 gas: 100 volume%, N2 gas: 0 volume%, CO gas: 0 volume%, H2 gas: 29 volume%, N2 gas: 71 volume%, CO gas: 0 volume% and H2 gas: 0 volume%, N2 gas: 37 volume%, CO gas: 63 volume%, including H2 gas in the range of 0 to 100 volume%, N2 gas in the range of 0 to 71 volume% and CO gas in the range of 0 to 100 volume%.
[0026] [4] The operating method of a blast furnace according to [2], wherein, when expressed in terms of the bosh gas composition, the high-concentration reducing gas is composed of H2 gas, N2 gas and CO gas, and the ratio of H2 gas, N2 gas and CO gas is a composition within an area surrounded by four points in the ternary phase diagram of H2 gas-N2 gas-CO gas: H2 gas: 0 volume%, N2 gas: 0 volume%, CO gas: 100 volume%, H2 gas: 100 volume%, N2 gas: 0 volume%, CO gas: 0 volume%, H2 gas: 29 volume%, N2 gas: 71 volume%, CO gas: 0 volume% and H2 gas: 0 volume%, N2 gas: 37 volume%, CO gas: 63 volume%, including H2 gas in the range of 0 to 100 volume%, N2 gas in the range of 0 to 71 volume% and CO gas in the range of 0 to 100 volume%.
[0027] [5] The method for operating a blast furnace according to any one of [1] to [4], wherein the amount of H2 gas in the high-concentration reducing gas is 0 to 500 Nm 3 / Hot metal-ton range.
[0028] Effects of the Invention
[0029] In the present invention, when a blast furnace operation is implemented to generate a high concentration of reducing gas in the furnace before the tuyere, the basicity (mass % CaO / mass % SiO2) of the total raw material components of the iron-based raw materials and the auxiliary raw materials is set within a specified range. As a result, the viscosity of the slag generated in the soft melting zone and the dripping zone in the blast furnace is optimized, and the liquid permeability of the slag in the blast furnace is controlled within an operable range. As a result, the gas permeability in the blast furnace can be maintained at a good level, and the stable operation of the blast furnace can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a diagram showing the composition range of the high-concentration reducing gas generated in the furnace before the tuyere by the blast furnace operating method of this embodiment in the gas component composition of the ternary phase diagram of H2 gas-N2 gas-CO gas as the bosh gas composition.
[0031] Figure 2 This is a graph showing the effect of the basicity of the total raw material components on the amount of melt dripping in an experiment in which a high-concentration reducing gas is generated in the furnace before the tuyere.
[0032] Figure 3 This is a graph showing the influence of the basicity of the total raw material component on the ventilation resistance index KS in a test in which a high-concentration reducing gas is generated in the furnace before the tuyere. DETAILED DESCRIPTION
[0033] Hereinafter, an embodiment of the present invention will be described. The method for operating a blast furnace of the present embodiment is a method for operating a blast furnace in which iron-based raw materials, auxiliary raw materials and coke are alternately and layeredly loaded into the blast furnace from the top of the blast furnace, gas is blown into the blast furnace from a tuyere arranged at the bottom of the blast furnace, and a high-concentration reducing gas is generated in the blast furnace in front of the tuyere by using the gas blown in from the tuyere. The iron-based raw materials include, for example, iron ore, sintered ore of iron ore, particles of iron ore, reduced iron and scrap iron. SiO2 and CaO are contained in the auxiliary raw materials alone or in combination. The types of the iron-based raw materials, auxiliary raw materials and coke used are not particularly limited, and as long as they are the iron-based raw materials, auxiliary raw materials and coke used in previous blast furnace operations, they can also be appropriately used in the present invention.
[0034] The gas used to generate the high-concentration reducing gas includes a reducing component that reduces the iron-based raw materials in the blast furnace. Here, the reducing component that reduces the iron-based raw materials in the blast furnace includes not only CO gas, H2 gas, and hydrocarbon gas as components that can reduce the iron-based raw materials, but also CO2 gas, H2O gas, etc. as components that generate reducing gas by reaction with coke or decomposition reaction.
[0035] Figure 1 It is a diagram showing the composition range of the high-concentration reducing gas generated in the furnace before the tuyere by the operating method of the blast furnace of this embodiment in the gas component composition of the ternary phase diagram of H2 gas-N2 gas-CO gas as a bosh gas composition. The high-concentration reducing gas in this embodiment refers to a reducing gas that achieves an average reduction rate of 80% or more when the iron-based raw material is reduced at 900°C for 180 minutes using the high-concentration reducing gas. When the reducing gas is represented by the bosh gas composition, it is composed of H2 gas, N2 gas and CO gas, and the ratio of H2 gas, N2 gas and CO gas (wherein the ratio is set to H2 gas + N2 gas + CO gas = 100% by volume) is in the range of Figure 1The range of region A (the operating range of the present invention) represented by the oblique line portion is a gas composition including H2 gas in the range of 0 to 100 volume %, N2 gas in the range of 0 to 71 volume %, and CO gas in the range of 0 to 100 volume %.
[0036] Region A is within the range surrounded by four points, namely, point O (H2 gas: 0 volume%, N2 gas: 0 volume%, CO gas: 100 volume%), point P (H2 gas: 100 volume%, N2 gas: 0 volume%, CO gas: 0 volume%), point Q (H2 gas: 29 volume%, N2 gas: 71 volume%, CO gas: 0 volume%), and point R (H2 gas: 0 volume%, N2 gas: 37 volume%, CO gas: 63 volume%), in the ternary phase diagram of H2 gas-N2 gas-CO gas. In addition, in Figure 1 1 shows the gas composition of the general blast furnace operation range in the past. In this region A, within the range surrounded by the four points of point O (H2 gas: 0 volume%, N2 gas: 0 volume%, CO gas: 100 volume%), point P (H2 gas: 100 volume%, N2 gas: 0 volume%, CO gas: 0 volume%), point Q' (H2 gas: 43 volume%, N2 gas: 57 volume%, CO gas: 0 volume%) and point R' (H2 gas: 0 volume%, N2 gas: 14 volume%, CO gas: 86 volume%), the average reduction rate when the iron-based raw material is reduced at 900°C for 180 minutes reaches more than 90%, so the FeO content in the slag component in the soft melting zone in the furnace is significantly reduced. Therefore, when a high-concentration reducing gas of this composition range is generated in the furnace of the tuyere, the effect of adjusting the basicity (mass%CaO / mass%SiO2) of the total raw material component for recovering the dripping amount of the molten material including the slag is further improved.
[0037] The inventors used a small test furnace simulating a 1 / 4 scale of a blast furnace to conduct an experiment to generate a high-concentration reducing gas in the furnace before the tuyere, and investigated the slag composition in the soft melting zone and dripping zone in the furnace. Table 1 shows an example of the composition of the iron-based raw materials used in the small test furnace.
[0038]
[0039] The following test was conducted in a small test furnace: the iron-based raw materials, auxiliary raw materials and coke were mixed in the same manner as the operation method described in Patent Document 2, with the basicity of the total raw material composition of the iron-based raw materials and auxiliary raw materials being 2.0, and a high-concentration reducing gas was generated in the furnace in front of the tuyere. Under the test conditions, the slag composition in the soft melting zone in the furnace was calculated to be: FeO composition less than 3.5% by mass, SiO2 composition 25.4-28.3% by mass, Al2O3 composition 8.6-9.2% by mass, CaO composition 52.5-56.7% by mass, and MgO composition 5.3-7.3% by mass. Since the basicity of the slag was as high as about 2.0 and the amount of slag dripping was reduced to about one-tenth of the previous test, the gas permeability deteriorated to a level beyond the range in which the test could be stably continued.
[0040] In order to increase the amount of slag dripping, it is considered necessary to reduce the basicity of the generated slag. Therefore, an experiment was conducted in which the basicity of the total raw material components of the iron-based raw materials and auxiliary raw materials was changed in the range of 0.95 to 2.23, and a high-concentration reducing gas was generated in the furnace in front of the tuyere to investigate the effect of the basicity of the total raw material components on the amount of molten material dripping and the ventilation resistance index KS.
[0041] Regarding the amount of melt dripping, the melt dripping during the test was recovered after the experiment, and its total weight was measured using a weighing instrument. The ventilation resistance index KS was calculated based on the integral value of the ventilation resistance K value (1 / m) calculated based on the pressure loss measured in the region where the temperature in the furnace is above 1000°C and the physical property values estimated based on the operating conditions.
[0042] <Calculation method of ventilation resistance index KS>
[0043] The ventilation resistance K value (1 / m) is calculated using the following formula (1).
[0044] K = (ΔP / H) / (ρ gas 0.7 ×μ gas 0.3 ×v gas 1.7 ) …(1)
[0045] Here, ΔP is the pressure loss (Pa), H is the thickness of the filling layer in the furnace (m), and ρ gas is the gas density (kg / m 3 ), μ gas is the gas viscosity (Pa·s), v gasis the gas flow rate (m / s). ΔP is obtained by installing a pressure gauge on the furnace wall at the tuyere and the upper part of the test furnace (the space above the filling layer) and calculating the pressure difference. Regarding H, for example, a measuring fixture is inserted through a hole punched in the upper part of the test furnace to measure the position of the filling layer surface, and the distance in the height direction between the filling layer surface position and the position where the tuyere is set is used as H. The position of the filling layer surface can be measured using a laser rangefinder. ρ gas It can be calculated from the gas composition introduced from the tuyere, the temperature in the furnace, and the pressure in the furnace. gas It can be calculated from the gas composition introduced from the tuyere and the temperature inside the furnace. gas It can be calculated from the gas flow rate introduced from the tuyere, the temperature in the furnace, and the pressure in the furnace. Here, regarding the temperature in the furnace, multiple thermometers are set on the furnace wall at a position corresponding to the filling layer, and the average value of the measured values of the thermometers is used. Similarly, regarding the pressure in the furnace, multiple thermometers are set on the furnace wall at a position corresponding to the filling layer, and the average value of the measured values of the pressure gauges is used. The average value of the pressure of the tuyere used in the calculation of ΔP and the pressure on the top of the filling layer can also be used as the pressure in the furnace.
[0046] The ventilation resistance index KS is calculated using the following formula (2).
[0047]
[0048] In the formula (2), Tmax is the maximum temperature at which the pressure loss in the furnace is measured, and it is different for each measurement, but is about 1500°C to about 1650°C.
[0049] Figure 2 This is a graph showing the effect of the basicity of the total raw material components on the amount of melt dripping in an experiment in which a high-concentration reducing gas is generated in the furnace before the tuyere. Figure 2 The horizontal axis is the basicity of the total raw material components (mass % CaO / mass % SiO2), and the vertical axis is the melt dripping amount (g).
[0050] Figure 3 This is a graph showing the influence of the basicity of the total raw material component on the ventilation resistance index KS in a test in which a high-concentration reducing gas is generated in the furnace before the tuyere. Figure 3 The horizontal axis is the basicity of the total raw material composition (mass% CaO / mass% SiO2), and the vertical axis is the ventilation resistance index KS (10 5 ℃ / m).
[0051] like Figure 2 As shown in FIG. 1 , when the basicity of the total raw material component of the iron-based raw material and the auxiliary raw material is in the range of 1.0 to 1.7, the amount of molten material dripping increases. Figure 3It is confirmed that when the basicity of the total raw material component of the iron-based raw material and the auxiliary raw material is in the range of 1.0 to 1.7, the ventilation resistance index KS decreases to below 2000, which is the target value. The target value of 2000 for the ventilation resistance index KS is the threshold value for continuous stable testing. A stable test is a test in which the surface height of the filling layer decreases uniformly over time and no faults such as blowby occur.
[0052] From these results, it was confirmed that by setting the basicity of the total raw material component of the iron-based raw material and the auxiliary raw material in the range of 1.0 to 1.7, it was possible to stably perform an experiment of generating a high-concentration reducing gas in the furnace before the tuyere.
[0053] The operating method of the blast furnace of the present embodiment is completed based on the above-mentioned test results. It is an operating method of the blast furnace in which iron-based raw materials, auxiliary raw materials and coke are charged from the top of the blast furnace and a high-concentration reducing gas is generated by blowing gas into the furnace in front of the tuyere from the blast furnace tuyere, wherein the alkalinity of the total raw material component of the charged iron-based raw materials and the charged auxiliary raw materials is set within a specified range.
[0054] Here, the basicity of the total raw material composition of the charged iron-based raw materials and the charged auxiliary raw materials is preferably within the range of 1.0 or more and 1.7 or less. This can improve the dripping property and air permeability of the molten material in the lower part of the blast furnace. When the basicity of the total raw material composition of the iron-based raw materials and the auxiliary raw materials is less than 1.0 and when the basicity of the total raw material composition of the iron-based raw materials and the auxiliary raw materials is greater than 1.7, the viscosity of the slag increases and is outside the stable operation range, so it is not preferred.
[0055] It should be noted that the basicity of the total raw material composition of the charged iron-based raw materials and auxiliary raw materials is more preferably 1.1 or more and 1.7 or less, and more preferably 1.4 or more and 1.5 or less. As a result, the viscosity of the slag is further reduced, and the dripping property and air permeability of the melt can be further improved. When adjusting the raw materials, it is preferred to set the slag amount to 400 kg / molten iron-ton or less. By setting the slag amount to 400 kg / molten iron-ton or less, the decrease in air permeability caused by the increase in the amount of melt melted out from the low temperature region can be suppressed.
[0056] In addition, the high-concentration reducing gas preferably has an H2 gas amount (including hydrogen in hydrocarbons) of 0 to 500 Nm 3 / molten iron-ton range. This can suppress the decrease in furnace temperature and the decrease in reduction reaction rate. On the other hand, the amount of H2 gas in the high-concentration reducing gas is greater than 500Nm 3 / molten iron-ton, the temperature in the furnace decreases and the reduction reaction rate decreases, so it is not preferred. In addition, when H2 gas is blown in as a single substance, in order to keep the temperature before the tuyere within the operating range, it is preferred to heat the H2 gas before blowing.
[0057] As described above, in the blast furnace operation method of the present embodiment, when the blast furnace operation is performed to generate high-concentration reducing gas in the furnace before the tuyere, the basicity of the total raw material components of the charged iron-based raw materials and the charged auxiliary raw materials is controlled within a specified range. As a result, the viscosity of the slag generated in the soft melting zone and the dripping zone in the blast furnace is optimized, the liquid permeability of the slag in the blast furnace is controlled within an operable range, and the gas permeability in the blast furnace can be maintained at a good level, thereby achieving stable operation.
[0058] Example
[0059] A large blast furnace was used to conduct the following blast furnace operation test: iron-based raw materials, auxiliary raw materials, and coke were alternately charged from the furnace top, the basicity of the total raw material composition of the iron-based raw materials and auxiliary raw materials charged from the furnace top was changed, and a high-concentration reducing gas was generated in the furnace in front of the tuyere. An example of the test results is shown in Table 2.
[0060]
[0061] As shown in Table 2, in Inventive Examples 1 to 4 in which the basicity of the total raw material component of the iron-based raw materials and auxiliary raw materials charged from the furnace top was set within the range of the present invention, it was confirmed that the dripping property and the air permeability were good and stable operation was possible. On the other hand, in Comparative Examples 1 to 3 in which the basicity of the total raw material component of the iron-based raw materials and auxiliary raw materials charged from the furnace top was outside the range of the present invention, sufficient dripping amount could not be obtained and the air permeability was also poor.
Claims
1. A method for operating a blast furnace, wherein an iron-based raw material, an auxiliary raw material and coke are charged from the top of the blast furnace and a gas is blown into the furnace from the tuyere to generate a high-concentration reducing gas in front of the tuyere, wherein: The basicity of the total raw material component of the iron-based raw material and the auxiliary raw material is set within a predetermined range.
2. The method for operating a blast furnace according to claim 1, wherein: The basicity of the total raw material components is set within a range of 1.0 to 1.
7.
3. The method for operating a blast furnace according to claim 1, wherein: When expressed in terms of the furnace bosh gas composition, the high-concentration reducing gas is composed of H2 gas, N2 gas and CO gas, and the ratio of H2 gas, N2 gas and CO gas is the composition within the area surrounded by four points in the ternary phase diagram of H2 gas-N2 gas-CO gas, namely, H2 gas: 0 volume%, N2 gas: 0 volume%, CO gas: 100 volume%, H2 gas: 100 volume%, N2 gas: 0 volume%, CO gas: 0 volume%, H2 gas: 29 volume%, N2 gas: 71 volume%, CO gas: 0 volume% and H2 gas: 0 volume%, N2 gas: 37 volume%, CO gas: 63 volume%, including H2 gas in the range of 0 to 100 volume%, N2 gas in the range of 0 to 71 volume% and CO gas in the range of 0 to 100 volume%.
4. The method for operating a blast furnace according to claim 2, wherein: When expressed in terms of the furnace bosh gas composition, the high-concentration reducing gas is composed of H2 gas, N2 gas and CO gas, and the ratio of H2 gas, N2 gas and CO gas is the composition within the area surrounded by four points in the ternary phase diagram of H2 gas-N2 gas-CO gas, namely, H2 gas: 0 volume%, N2 gas: 0 volume%, CO gas: 100 volume%, H2 gas: 100 volume%, N2 gas: 0 volume%, CO gas: 0 volume%, H2 gas: 29 volume%, N2 gas: 71 volume%, CO gas: 0 volume% and H2 gas: 0 volume%, N2 gas: 37 volume%, CO gas: 63 volume%, including H2 gas in the range of 0 to 100 volume%, N2 gas in the range of 0 to 71 volume% and CO gas in the range of 0 to 100 volume%.