Exterior member and method for manufacturing same

By precipitating metal hydroxides and oxides in the anodized film of aluminum or aluminum alloy exterior components and compounding them with silicate or acrylic organics, the problems of acid resistance and alkali resistance reduction caused by heating treatment are solved, and the problem of acid resistance and alkali resistance reduction is achieved. The effect of significantly improving acid resistance and alkali resistance.

CN119032202APending Publication Date: 2024-11-26AISIN KEIKINZOKU CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280094398.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2022-10-28
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During heat treatment, existing aluminum or aluminum alloy exterior components cause cracks to occur due to different thermal expansion rates, which reduce their acid resistance and alkali resistance.

Method used

By precipitating metal hydroxides and metal oxides in the fine pores of the anodized coating, forming a composite film layer, and recombining it with silicate or acrylic organic substances on its surface, improving acid resistance and alkali resistance. The specific steps include forming an anodized layer on the surface of aluminum or aluminum alloy, sealing the pores using an aqueous solution containing nickel fluoride and zirconium fluoric acid, and then impregnating the solution in an aqueous solution containing silicate and acrylic organic matter.

Benefits of technology

The acid resistance and alkali resistance of aluminum or aluminum alloy exterior components have been significantly improved. The composite film layer of the anodized cover can remain stable under high temperature and high pressure environment, and has excellent acid resistance and alkali resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032202A_ABST
    Figure CN119032202A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide: an exterior member having excellent acid and alkali resistance; and a method for producing the exterior member. The present invention relates to a metal material comprising aluminum or an aluminum alloy, and an anodized layer formed on the surface of the metal material, the anodized layer having countless micropores, and a composite film layer of a metal hydroxide and a metal oxide on the surface side of the micropores.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to various exterior components using aluminum or aluminum alloy as raw materials and methods for producing the same, and in particular to exterior components such as automobile exterior components that require acid resistance and alkali resistance. Background Art

[0002] Conventionally, anodizing treatment has been performed for the purpose of rust prevention of various products used as raw materials such as aluminum or aluminum alloys.

[0003] This anodic oxide film is composed of a porous layer having numerous fine pores with an inner diameter of about 5 to 30 nm formed on a barrier layer with a thickness of about 10 to 20 nm.

[0004] Since the micropores of the anodic oxide film themselves have insufficient corrosion resistance, a so-called sealing treatment is performed.

[0005] As a sealing treatment, it is known that in a boehmite treatment based on a hot water treatment at 90°C or above, a steam treatment, etc., the corrosion resistance is insufficient or turbidity may be generated on the surface. Therefore, there are known high-temperature sealing treatment methods in which nickel hydroxide is precipitated in micropores by treating with a nickel acetate-based aqueous solution in hot water at a relatively high temperature of 80°C or above, combined with boehmite treatment of aluminum oxide, and a method in which nickel hydroxide and aluminum fluoride are compositely precipitated at a relatively low temperature of room temperature to 40°C using a nickel fluoride-based aqueous solution.

[0006] In Patent Document 1, a sealed anodic oxide film is described for the purpose of further improving the resistance to steam and to alkali and acid. The sealed anodic oxide film is composed of an anode region filled with at least one of crystalline transition metal oxides, crystalline precious metal oxides, semi-metal oxides, alkaline earth metal oxides and alkali metal oxides and a sealing region containing at least one of them.

[0007] Specifically, according to this embodiment, the anodized aluminum substrate is heat-treated at about 150° C. to about 300° C. for about 30 minutes to about 2 hours to at least partially crystallize it.

[0008] However, there is a large difference in thermal expansion coefficient between aluminum metal materials and inorganic materials such as anodized films. During heat treatment, numerous cracks are generated in the anodized film, which may cause a decrease in acid and alkali resistance.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application No. 2013-528707 Summary of the invention

[0012] Technical problem to be solved by the invention

[0013] An object of the present invention is to provide an exterior member having excellent acid and alkali resistance and a method for producing the same.

[0014] Technical solutions for solving technical problems

[0015] The exterior component involved in the present invention is characterized in that it has a metal material composed of aluminum or aluminum alloy and an anodized layer formed on the surface of the metal material, the anodized layer has countless micropores, and a composite film layer of metal hydroxide and metal oxide is provided on the surface side of the micropores.

[0016] In the present invention, as a sealing treatment for the anodic oxide film, metal hydroxide and metal oxide are precipitated in micropores to form a composite film layer, thereby achieving both alkali resistance due to the metal hydroxide and acid resistance due to the metal oxide.

[0017] In the anodized film, aluminum oxide formed during anodization forms boehmite (monohydrate) or bayerite (trihydrate) through a hydration reaction, but these hydrates may be composited with metal hydroxides and metal oxides.

[0018] In the present invention, examples of the metal hydroxide include nickel hydroxide, zirconium hydroxide, cobalt hydroxide, zinc hydroxide, and vanadium hydroxide.

[0019] In addition, examples of metal oxides include zirconium oxide, titanium oxide, and the like.

[0020] In the present invention, the composite film layer preferably contains at least nickel hydroxide and zirconium oxide or zirconium hydroxide.

[0021] In the present invention, if one or both of a silicate and an acrylic organic substance having a high affinity with the metal oxide precipitated in the micropores are further compounded, the acid resistance and the alkali resistance are further improved.

[0022] Here, silicate refers to a silicic acid compound having orthosilicate ions, pyrosilicate ions, or the like as a skeleton.

[0023] In addition, acrylic organic matter refers to resin components such as polyacrylic acid and copolymerized acrylic acid, which enter the gaps between inorganic precipitates to improve acid resistance and alkali resistance.

[0024] The method for manufacturing an exterior member according to the present invention comprises: forming an anodic oxide layer having numerous fine pores on the surface of a metal material composed of aluminum or an aluminum alloy; reacting with an aqueous solution containing nickel fluoride and zirconium fluoride acid; and reacting with an aqueous solution containing a silicate.

[0025] Here, when nickel fluoride is precipitated in the micropores, it is precipitated as nickel hydroxide, and when zirconium fluoride is precipitated in the micropores, it is precipitated as zirconium oxide or zirconium hydroxide.

[0026] Nickel fluoride may also be a tetrahydrate such as F2Ni·4H2O. Fluorozirconic acid is also called hydrofluoriczirconate or hydrofluoriczirconic acid and is represented by H2ZrF6.

[0027] Furthermore, the aqueous solution may contain nickel acetate, potassium fluoride, a surfactant, and the like.

[0028] In the present invention, the aqueous solution containing the silicate may contain an acrylic acid-based organic substance together with a surfactant.

[0029] Effects of the Invention

[0030] In the exterior member of the present invention, the anodic oxide film is sealed to form a composite film layer of metal hydroxide and metal oxide, thereby achieving excellent acid resistance and alkali resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The evaluation results are shown.

[0032] Figure 2 A method for measuring the thickness of a composite film layer is shown.

[0033] Figure 3 Shows the element mapping image, Figure 3 (a) represents Si, Figure 3 (b) represents Ni, Figure 3 (c) represents Al. DETAILED DESCRIPTION

[0034] Test pieces were prepared, and the alkali resistance and acid resistance were evaluated and described below, but the present invention is not limited thereto.

[0035] Example 1

[0036] (1) A 200 g / L sulfuric acid aqueous solution was used for the aluminum plate at 20°C and a current density of 1 A / dm 2 The electrolytic treatment was carried out for 30 minutes to form an anodic oxide film of about 9 μm, which was then thoroughly washed with water.

[0037] (2) Next, the samples were immersed in an aqueous solution containing 0.55% nickel fluoride (tetrahydrate), 0.5% nickel acetate, 0.05% zirconium fluoride, 0.04% potassium fluoride, and 0.2% or less of a surfactant in the following mass % at 75°C for 15 minutes, and then thoroughly washed with water.

[0038] (3) Next, the film is immersed in an aqueous solution containing about 0.1% silicate, about 0.1% acrylic acid organic matter, and 0.1-0.2% surfactant at about 95°C for 20 minutes, and then thoroughly rinsed with water.

[0039] (4) Regarding the thickness of the composite film layer formed on the surface side of the anodized film, Figure 2 As shown, when the surface treated portion is bent, the fracture surface of the anodized film is exposed.

[0040] The observation was performed using JSM-IT700HR manufactured by JEOL Ltd. at a magnification of 35,000 times, and the thickness from the upper surface to the point where columnar micropores of the anodic oxide film could be confirmed was defined as the composite film layer.

[0041] In Example 1, it is about 300 nm.

[0042] (5) shows a TEM element mapping image of Si, Ni, and Al near the surface of the anodic oxide film.

[0043] This shows that the composite membrane layer is composed of a portion filled in the micropores and a layer precipitated on the surface thereof.

[0044] Example 2

[0045] Example 2 In Example 1, the first-stage treatment time shown in (2) was set to 10 minutes, and the second-stage treatment time shown in (3) was set to 15 minutes.

[0046] The other parts were prepared in the same manner as in Example 1.

[0047] The thickness of the composite film layer is about 200 nm.

[0048] Reference Example 1

[0049] In Reference Example 1, the first-stage treatment condition described in (2) of Example 1 was set to 5 minutes, and the second-stage treatment condition described in (3) was set to 10 minutes.

[0050] The other parts were prepared in the same manner as in Example 1.

[0051] The thickness of the composite film layer is about 100 nm.

[0052] Comparative Example 1

[0053] Comparative Example 1 After forming an anodic oxide film in the same manner as in Example 1 (1), a sealing treatment was performed at 90° C. for 20 minutes using a 0.5% nickel acetate aqueous solution.

[0054] Comparative Example 2

[0055] Comparative Example 2 After forming an anodic oxide film in the same manner as in Example 1 (1), a first-stage sealing treatment was performed at 30° C. for 20 minutes using an approximately 3% nickel fluoride aqueous solution, and then, as a second stage, steam pore removal was performed for 20 minutes.

[0056] Using the test pieces prepared in Examples 1 and 2, Reference Example 1, and Comparative Examples 1 and 2, alkali resistance and acid resistance tests were carried out as follows.

[0057] <Alkali resistance test method>

[0058] The sample was immersed in a sodium hydroxide aqueous solution having a pH of 12.5 at room temperature for 10 minutes, and then washed and dried.

[0059] The gloss before and after the test was measured using a HORIBA IG-410 gloss meter, and the gloss retention rate was calculated by the following formula (1).

[0060] Gloss retention rate (%) = gloss after test / gloss before test × 100 … (1)

[0061] <Acid resistance test method>

[0062] One drop of a pH 4 sulfuric acid aqueous solution was added to the test piece, and after drying, one drop of a pH 4 sulfuric acid aqueous solution was repeatedly added to the same position.

[0063] The dripping portion was wiped with a wet paper towel, and the number of drippings until the portion turned white was counted.

[0064] The evaluation results are shown in Figure 1 of table.

[0065] Compared with Comparative Examples 1 and 2, Examples 1 and 2 are superior in both alkali resistance and acid resistance.

[0066] If the present invention is applied to automobile exterior parts, the gloss retention rate is targeted to be 80% or more and the acid resistance is 200 times or more.

[0067] The acid resistance of Reference Example 1 is also better than that of Comparative Examples 1 and 2. Therefore, although the effect of the present invention is confirmed, when the composite film thickness is as thin as 100nm, the alkali resistance and acid resistance are worse than those of Examples 1 and 2. Therefore, the composite film thickness is preferably greater than 200nm.

[0068] <Comparison with existing technologies>

[0069] Based on the test piece of Example 1 in the present invention and paragraph (0051) of Patent Document 1, the applicant prepared a test piece and carried out an immersion test in a pH 0.8 sulfuric acid aqueous solution for 24 hours.

[0070] In Example 1 of the present application, the reduction rate of the film thickness was less than 5%, whereas that of the additional test sample of Patent Document 1 was reduced by about 20%.

[0071] Therefore, it is estimated that the exterior member according to the present invention has higher acid resistance than the conventional one.

[0072] In this embodiment, the processing conditions are not limited to those of Embodiments 1 and 2.

[0073] For example, the purpose of the first-stage treatment liquid is to precipitate nickel hydroxide and zirconium oxide or zirconium hydroxide in micropores, and the composition is preferably in the following range in terms of mass %.

[0074] (1) Nickel fluoride: 0.30~1.00%

[0075] (2) Zirconium fluoride: 0.02~0.05%

[0076] (3) Potassium fluoride: less than 0.05%

[0077] The second-stage treatment liquid preferably contains 0.05-0.20% silicate, 0.05-0.20% acrylic acid organic matter, and 0.20% or less of surfactant.

[0078] Industrial Applicability

[0079] The exterior member using the aluminum alloy according to the present invention as a raw material has excellent both acid resistance and alkali resistance and can be used for various exterior parts including automobile exterior members.

Claims

1. An exterior component, characterized in that: The exterior member includes a metal material made of aluminum or an aluminum alloy and an anodized layer formed on a surface of the metal material. The anodized layer has numerous micropores and has a composite film layer of metal hydroxide and metal oxide on the surface side of the micropores.

2. The exterior member according to claim 1, characterized in that: The composite film layer at least contains nickel hydroxide and zirconium oxide or zirconium hydroxide.

3. The exterior member according to claim 2, characterized in that: The composite film layer further comprises silicate.

4. The exterior member according to claim 3, characterized in that: The composite film layer further contains acrylic acid-based organic matter.

5. The exterior member according to any one of claims 1 to 4, characterized in that: The thickness of the composite film layer is greater than 200 nm.

6. A method for manufacturing an exterior member, characterized in that: The manufacturing method has the following features: A step of forming an anodic oxide layer having numerous fine pores on the surface of a metal material composed of aluminum or an aluminum alloy; A step of reacting with an aqueous solution containing nickel fluoride and fluorozirconic acid; as well as A step of reacting with an aqueous solution containing a silicate.

7. The method for manufacturing an exterior member according to claim 6, characterized in that: The aqueous solution containing the silicate contains an acrylic acid-based organic substance.