Inorganic compound-starch co-treatment pregelatinization auxiliary material as well as preparation method and application thereof

The pregelatinized auxiliary materials for the preparation of inorganic compounds-starch by microwave treatment were solved, and the preparation process of cumbersome and high cost in the existing technology was achieved, and the preparation process was simplified and the preparation process was improved and the properties of the powder were improved. Effect.

CN119033945AActive Publication Date: 2024-11-29ANHUI UNIVERSITY OF TRADITIONAL CHINESE MEDICINE

Patent Information

Application Number
CN202411082350.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-29
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The existing method of pregelatinized starch and inorganic salt is cumbersome in preparation, energy consumption, resulting in high production costs and high equipment requirements, making it difficult to take into account the functions of both.

Method used

The microwave treatment method is used to mix the pharmaceutical inorganic salts and/or pharmaceutical inorganic oxides with starch, and the microwave energy value is controlled between 1310J~21840J/g of starch, and the inorganic compound-starch co-treated pregelatinized auxiliary materials are obtained, which simplifies the preparation process. And reduce equipment requirements.

Benefits of technology

This method simplifies the preparation process, reduces production costs, improves the powdery properties and the application of the preparation, retains the functions of pregelatinized starch and inorganic compounds, and improves the fluidity and compressibility of the powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119033945A_ABST
    Figure CN119033945A_ABST
Patent Text Reader

Abstract

The invention discloses an inorganic compound-starch co-treatment pregelatinization auxiliary material as well as a preparation method and application thereof. The preparation method comprises the following steps: mixing medicinal inorganic salt and / or medicinal inorganic oxide with water, and then mixing with starch; placing the mixed system in a microwave reactor for microwave treatment; and drying the microwave treatment product. According to the invention, the mixed system of the starch and the medicinal inorganic salt and / or the medicinal inorganic oxide is subjected to pregelatinization treatment for the first time to obtain the inorganic compound-starch co-treated pregelatinized auxiliary material, so that the corresponding functions of the pregelatinized starch and the inorganic compound as medicinal auxiliary materials are reserved; the flowability and compressibility of the powder and the disintegration performance of a solid preparation prepared from the powder are improved. The preparation method is simple in process and low in equipment requirement, and the prepared co-processing auxiliary material can be used as a whole and used as a raw material for dry / wet granulation and direct powder compression, so that the preparation method has important significance in simplifying production steps, improving production efficiency and reducing production cost for enterprises.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pharmaceutical excipients, and particularly relates to an inorganic compound-starch co-processed pregelatinized excipient and a preparation method and application thereof. Background Art

[0002] Pregelatinized starch is a pharmaceutical excipient prepared by modifying starch by chemical or physical methods. Compared with starch, pregelatinized starch has good fluidity and compressibility and can be used as an excipient for direct powder tableting. Inorganic salts, as an important pharmaceutical excipient, are often used in combination with pregelatinized starch in tablet formulations.

[0003] At present, the method of combining the two is mainly to first prepare pregelatinized starch by wet heat method, mechanical activation method, ethanol-alkali method and microwave method, and then physically mix the pregelatinized starch with inorganic salts and other ingredients, and press the pregelatinized starch into tablets after dry or wet granulation or directly press the powder into tablets. The preparation method of pregelatinized starch takes a long time, consumes a lot of energy, is complicated to prepare, has high equipment requirements, and has high production costs for enterprises.

[0004] Considering the application scenarios of pregelatinized starch and inorganic salts, exploring a method for preparing a mixed auxiliary material that can combine the functions of these two raw materials and is easy to use has become a problem that needs to be solved urgently in this field. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides an inorganic compound-starch co-processed pregelatinized auxiliary material and a preparation method and application thereof. The co-processed pregelatinized auxiliary material retains the respective functions of pregelatinized starch and the inorganic compound, while improving the powder properties of the prepared powder and improving the applicability of the preparation. The preparation method is simple, which is conducive to reducing production costs.

[0006] The first aspect of the present invention provides a method for preparing an inorganic compound-starch co-processed pregelatinized auxiliary material, comprising: mixing a medicinal inorganic salt and / or a medicinal inorganic oxide with water, and then mixing with starch; placing the mixed system in a microwave reactor for microwave treatment; and drying the microwave-treated product. The order of mixing the medicinal inorganic salt and / or the medicinal inorganic oxide with water and starch is important. If starch and water are mixed first, the overall viscosity of the liquid will increase. After the medicinal inorganic salt and / or the medicinal inorganic oxide are added, the medicinal inorganic salt and / or the medicinal inorganic oxide may not be mixed evenly with the starch due to the increased resistance of the liquid.

[0007] According to a specific embodiment of the present invention, the mass ratio of the medicinal inorganic salt and / or medicinal inorganic oxide, water and starch is 1:4-16:0.25-5.

[0008] According to a specific embodiment of the present invention, the pharmaceutically acceptable inorganic salt is selected from sodium carbonate, calcium carbonate, calcium hydrogen phosphate dihydrate, tricalcium phosphate or calcium sulfate dihydrate.

[0009] According to a specific embodiment of the present invention, the pharmaceutically acceptable inorganic oxide is silicon dioxide.

[0010] According to a specific embodiment of the present invention, the starch is selected from corn starch, potato starch or wheat starch.

[0011] According to a specific embodiment of the present invention, during the microwave treatment, the time and frequency of the microwave treatment are adjusted so that the microwave energy value obtained per gram of starch is 1310J to 21840J.

[0012] The second aspect of the present invention provides an inorganic compound-starch co-processed pregelatinized auxiliary material prepared according to the aforementioned method.

[0013] The third aspect of the present invention provides a pharmaceutical preparation containing the aforementioned inorganic compound-starch co-processed pregelatinized excipient.

[0014] The fourth aspect of the present invention provides the use of the aforementioned inorganic compound-starch co-processed pregelatinized auxiliary material in dry or wet granulation.

[0015] The fifth aspect of the present invention provides the use of the aforementioned inorganic compound-starch co-processed pregelatinized auxiliary material in direct powder tableting.

[0016] The beneficial effects of the present invention are:

[0017] The preparation method provided by the present invention pregelatinizes the mixed system of starch and medicinal inorganic salts and / or medicinal inorganic oxides for the first time to obtain an inorganic compound-starch co-processed pregelatinized auxiliary material, which not only retains the corresponding functions of the pregelatinized starch and the inorganic compound as pharmaceutical auxiliary materials, but also improves the fluidity and compressibility of the powder and the disintegration performance of the solid preparation prepared by the same. The preparation method has a simple process and low equipment requirements. The prepared co-processed auxiliary material can be used as a whole as a raw material for dry / wet granulation and direct compression of powders, which is of great significance for enterprises to simplify production steps, improve production efficiency and reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The scanning electron microscope images of the samples, A: the sample of Example 1; B: the sample of Example 2. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. In the embodiments of the present invention, the methods used are conventional methods unless otherwise specified, and the reagents used can be obtained from commercial channels.

[0020] The present invention provides a method for preparing a medicinal inorganic salt / or medicinal inorganic oxide-starch co-processed pregelatinized auxiliary material, wherein a mixture of medicinal inorganic salt / or medicinal inorganic oxide and starch auxiliary material is formed in a certain proportion, and the mixture is processed under different microwave conditions (the microwave energy value obtained per gram of starch is controlled to be 1310J-21840J) to obtain the co-processed pregelatinized auxiliary material with different pregelatinization degrees. The calculation formula of microwave energy is: the microwave energy value obtained per gram of starch = microwave power output rate (%) × output power (%) × energy conversion efficiency (%) × microwave processing time (s) / starch mass (g).

[0021] Example 1

[0022] A sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 1310 -The preparation method of SC1MS1-UW4 comprises the following steps:

[0023] (1) Preparation of sodium carbonate solution SC1-UM4: According to the mass ratio of sodium carbonate to ultrapure water of 1:4, weighed sodium carbonate and ultrapure water were stirred and mixed uniformly at room temperature to prepare sodium carbonate solution SC1-UM4.

[0024] (2) Preparation of corn starch suspension SC1MS1-UM4 containing sodium carbonate: According to the mass ratio of sodium carbonate to corn starch of 1:1, the weighed corn starch is added to the sodium carbonate solution of step (1), and the mixture is stirred and mixed evenly at room temperature. The mixture is sealed with plastic wrap to prevent water loss, and the corn starch suspension SC1MS1-UM4 containing sodium carbonate is obtained.

[0025] (3) Sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 1310 - Preparation of SC1MS1-UW4: The corn starch suspension containing sodium carbonate prepared in step (2) is placed in a microwave reactor for treatment, and the microwave energy value obtained per gram of corn starch is controlled to be 1310J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, microwave treatment for 1 minute and stirring for 10 seconds until the microwave treatment is completed. Then, the prepared pregelatinized corn starch system containing sodium carbonate is freeze-dried to obtain a sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT.1310 -SC1MS1-UW4.

[0026] Example 2

[0027] A sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 21840 -The preparation method of SC1MS1-UW4 comprises the following steps:

[0028] (1) Preparation of sodium carbonate solution SC1-UM4: According to the mass ratio of sodium carbonate to ultrapure water being 1:4, weighed sodium carbonate and ultrapure water were stirred and mixed uniformly at room temperature to prepare sodium carbonate solution SC1-UM4.

[0029] (2) Preparation of corn starch suspension SC1MS1-UM4 containing sodium carbonate: According to the mass ratio of sodium carbonate to corn starch of 1:1, the weighed corn starch is added to the sodium carbonate solution of step (1), and the mixture is stirred and mixed evenly at room temperature. The mixture is sealed with plastic wrap to prevent water loss, and the corn starch suspension SC1MS1-UM4 containing sodium carbonate is obtained.

[0030] (3) Sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 21840 - Preparation of SC1MS1-UW4: The corn starch suspension containing sodium carbonate prepared in step (2) is placed in a microwave reactor for reaction, and the energy value obtained per gram of corn starch is controlled to be 21840 J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1 min and stirred for 10 s until the microwave treatment is completed. Then, the prepared pregelatinized corn starch system containing sodium carbonate is freeze-dried to obtain a sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT. 21840 -SC1MS1-UW4.

[0031] Example 3

[0032] MT of a sodium carbonate-corn starch co-processed pregelatinized auxiliary material 1310 -SC1MS5-UW4 preparation method, comprising the following steps:

[0033] (1) Preparation of sodium carbonate solution SC1-UM4: According to the mass ratio of sodium carbonate to ultrapure water being 1:4, weighed sodium carbonate and ultrapure water were stirred and mixed uniformly at room temperature to prepare sodium carbonate solution SC1-UM4.

[0034] (2) Preparation of corn starch suspension SC1MS5-UW4 containing sodium carbonate: according to the mass ratio of sodium carbonate to corn starch of 1:5, the weighed corn starch is added to the sodium carbonate solution of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss.

[0035] (3) Sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 1310 - Preparation of SC1MS5-UW4: The corn starch suspension containing sodium carbonate prepared in step (2) is placed in a microwave reactor for treatment, and the energy value obtained per gram of corn starch is controlled to be 1310J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1min and stirred for 10s until the microwave is finished. Then, the prepared pregelatinized corn starch system containing sodium carbonate is freeze-dried to obtain a sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT. 1310 -SC1MS5-UW4.

[0036] Example 4

[0037] A sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 21840 -The preparation method of SC1MS5-UW4 comprises the following steps:

[0038] (1) Preparation of sodium carbonate solution SC1-UM4: According to the mass ratio of sodium carbonate to ultrapure water being 1:4, weighed sodium carbonate and ultrapure water were stirred and mixed uniformly at room temperature to prepare sodium carbonate solution SC1-UM4.

[0039] (2) Preparation of corn starch suspension SC1MS5-UW4 containing sodium carbonate: according to the mass ratio of sodium carbonate to corn starch of 1:5, the weighed corn starch is added to the sodium carbonate solution of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss.

[0040] (3) Sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 21840 - Preparation of SC1MS5-UW4: The corn starch suspension containing sodium carbonate prepared in step (2) is placed in a microwave reactor for treatment, and the energy value obtained per gram of corn starch is controlled to be 21840 J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1 min, and stirring is performed for 10 s until the microwave is finished. Then, the prepared pregelatinized corn starch system containing sodium carbonate is freeze-dried to obtain a sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT. 21840 -SC1MS5-UW4.

[0041] Example 5

[0042] A sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 1310 -The preparation method of SC1MS1-UW8 comprises the following steps:

[0043] (1) Preparation of sodium carbonate solution SC1-UM8: According to the mass ratio of sodium carbonate to ultrapure water being 1:8, weighed sodium carbonate and ultrapure water were stirred and mixed evenly at room temperature to prepare sodium carbonate solution SC1-UM8.

[0044] (2) Preparation of corn starch suspension SC1MS1-UW8 containing sodium carbonate: According to the mass ratio of sodium carbonate to corn starch of 1:1, the weighed corn starch is added to the sodium carbonate solution of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss.

[0045] (3) Sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 1310 - Preparation of SC1MS1-UW8: The corn starch suspension containing sodium carbonate prepared in step (2) is placed in a microwave reactor for treatment, and the energy value obtained per gram of corn starch is controlled to be 1310J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1min and stirred for 10s until the microwave is finished. Then, the prepared pregelatinized corn starch system containing sodium carbonate is freeze-dried to obtain a sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT. 1310 -SC1MS1-UW8.

[0046] Example 6

[0047] A sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 21840 -The preparation method of SC1MS1-UW8 comprises the following steps:

[0048] (1) Preparation of sodium carbonate solution SC1-UM8: According to the mass ratio of sodium carbonate to ultrapure water being 1:8, weighed sodium carbonate and ultrapure water were stirred and mixed evenly at room temperature to prepare sodium carbonate solution SC1-UM8.

[0049] (2) Preparation of corn starch suspension SC1MS1-UW8 containing sodium carbonate: According to the mass ratio of sodium carbonate to corn starch of 1:1, the weighed corn starch is added to the sodium carbonate solution of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss.

[0050] (3) Sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 21840- Preparation of SC1MS1-UW8: The corn starch suspension containing sodium carbonate prepared in step (2) is placed in a microwave reactor for treatment, and the energy value obtained per gram of corn starch is controlled to be 21840 J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1 min, and stirring is performed for 10 s until the microwave is finished. Then, the prepared pregelatinized corn starch system containing sodium carbonate is freeze-dried to obtain a sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT. 21840 -SC1MS1-UW8.

[0051] Example 7

[0052] A sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 1310 -The preparation method of SC1MS5-UW8 comprises the following steps:

[0053] (1) Preparation of sodium carbonate solution SC1-UM8: According to the mass ratio of sodium carbonate to ultrapure water being 1:8, weighed sodium carbonate and ultrapure water were stirred and mixed evenly at room temperature to prepare sodium carbonate solution SC1-UM8.

[0054] (2) Preparation of corn starch suspension SC1MS5-UW8 containing sodium carbonate: According to the mass ratio of sodium carbonate to corn starch of 1:5, the weighed corn starch is added to the sodium carbonate solution of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss.

[0055] (3) Sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 1310 - Preparation of SC1MS5-UW8: The corn starch suspension containing sodium carbonate prepared in step (2) is placed in a microwave reactor for treatment, and the energy value obtained per gram of corn starch is controlled to be 1310J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1min and stirred for 10s until the microwave is finished. Then, the prepared pregelatinized corn starch system containing sodium carbonate is freeze-dried to obtain a sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT. 1310 -SC1MS5-UW8.

[0056] Example 8

[0057] A sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 21840 -The preparation method of SC1MS5-UW8 comprises the following steps:

[0058] (1) Preparation of sodium carbonate solution SC1-UM8: According to the mass ratio of sodium carbonate to ultrapure water being 1:8, weighed sodium carbonate and ultrapure water were stirred and mixed evenly at room temperature to prepare sodium carbonate solution SC1-UM8.

[0059] (2) Preparation of corn starch suspension SC1MS5-UW8 containing sodium carbonate: According to the mass ratio of sodium carbonate to corn starch of 1:5, the weighed corn starch is added to the sodium carbonate solution of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss.

[0060] (3) Sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT 21840 - Preparation of SC1MS5-UW8: The corn starch suspension containing sodium carbonate prepared in step (2) is placed in a microwave reactor for treatment, and the energy value obtained per gram of corn starch is controlled to be 21840 J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1 min, and stirring is performed for 10 s until the microwave is finished. Then, the prepared pregelatinized corn starch system containing sodium carbonate is freeze-dried to obtain a sodium carbonate-corn starch co-processed pregelatinized auxiliary material MT. 21840 -SC1MS5-UW8.

[0061] Example 9

[0062] A pregelatinized auxiliary material MT of calcium hydrogen phosphate dihydrate and corn starch co-processing 1310 -The preparation method of DCPD1MS1-UW4 comprises the following steps:

[0063] (1) Preparation of dihydrate calcium hydrogen phosphate suspension DCPD1-UW4: According to the mass ratio of dihydrate calcium hydrogen phosphate to ultrapure water of 1:4, weighed dihydrate calcium hydrogen phosphate and ultrapure water were stirred and mixed uniformly at room temperature to prepare dihydrate calcium hydrogen phosphate suspension DCPD1-UW4.

[0064] (2) Preparation of corn starch suspension DCPD1MS1-UW4 containing dibasic calcium phosphate dihydrate: according to the mass ratio of dibasic calcium phosphate dihydrate to corn starch of 1:1, the weighed corn starch is added to the dibasic calcium phosphate dihydrate suspension of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss, to obtain corn starch suspension DCPD1MS1-UW4 containing dibasic calcium phosphate dihydrate.

[0065] (3) Calcium hydrogen phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT 1310Preparation of -DCPD1MS1-UW4: The corn starch suspension containing dihydrogen calcium phosphate dihydrate prepared in step (2) is placed in a microwave reactor for treatment, and the microwave energy value obtained per gram of corn starch is controlled to be 1310J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is adopted, that is, microwave treatment for 1 minute and stirring for 10 seconds until the microwave treatment is completed. Then, the prepared pregelatinized corn starch system containing dihydrogen calcium phosphate dihydrate is dried to obtain a dihydrogen calcium phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT. 1310 -DCPD1MS1-UW4.

[0066] Example 10

[0067] A pregelatinized auxiliary material MT of calcium hydrogen phosphate dihydrate and corn starch co-processing 21840 -The preparation method of DCPD1MS1-UW4 comprises the following steps:

[0068] (1) Preparation of dihydrate calcium hydrogen phosphate suspension DCPD1-UW4: According to the mass ratio of dihydrate calcium hydrogen phosphate to ultrapure water being 1:4, the weighed dihydrate calcium hydrogen phosphate and ultrapure water were stirred and mixed uniformly at room temperature to prepare dihydrate calcium hydrogen phosphate suspension DCPD1-UW4.

[0069] (2) Preparation of corn starch suspension DCPD1MS1-UW4 containing dibasic calcium phosphate dihydrate: according to the mass ratio of dibasic calcium phosphate dihydrate to corn starch of 1:1, the weighed corn starch is added to the dibasic calcium phosphate dihydrate suspension of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss, to obtain corn starch suspension DCPD1MS1-UW4 containing dibasic calcium phosphate dihydrate.

[0070] (3) Calcium hydrogen phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT 21840 Preparation of -DCPD1MS1-UW4: Place the corn starch suspension containing dihydrogen calcium phosphate dihydrate prepared in step (2) in a microwave reactor for reaction, and control the energy value obtained per gram of corn starch to be 21840J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1min and stirred for 10s until the microwave treatment is completed. Then, the prepared pregelatinized corn starch system containing dihydrogen calcium phosphate dihydrate is freeze-dried to obtain a dihydrogen calcium phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT. 21840 -DCPD1MS1-UW4.

[0071] Embodiment 11

[0072] MT of a pregelatinized auxiliary material co-processed with calcium hydrogen phosphate dihydrate and corn starch 1310 -DCPD1MS 0.25-UW4 preparation method, comprising the following steps:

[0073] (1) Preparation of dihydrate calcium hydrogen phosphate suspension DCPD1-UW4: According to the mass ratio of dihydrate calcium hydrogen phosphate to ultrapure water being 1:4, the weighed dihydrate calcium hydrogen phosphate and ultrapure water were stirred and mixed uniformly at room temperature to prepare dihydrate calcium hydrogen phosphate suspension DCPD1-UW4.

[0074] (2) Corn starch suspension containing dibasic calcium phosphate dihydrate DCPD1MS 0.25 - Preparation of UW4: According to the mass ratio of dihydrate calcium phosphate to corn starch of 1:0.25, the weighed corn starch is added to the dihydrate calcium phosphate suspension of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss.

[0075] (3) Calcium hydrogen phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT 1310 -DCPD1MS 0.25 Preparation of -UW4: The corn starch suspension containing dihydrogen calcium phosphate dihydrate prepared in step (2) is placed in a microwave reactor for treatment, and the energy value obtained per gram of corn starch is controlled to be 1310J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1min and stirred for 10s until the microwave is finished. Then, the prepared pregelatinized corn starch system containing dihydrogen calcium phosphate dihydrate is freeze-dried to obtain a dihydrogen calcium phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT. 1310 -DCPD1MS 0.25 -UW4.

[0076] Example 12

[0077] A pregelatinized auxiliary material MT of calcium hydrogen phosphate dihydrate and corn starch co-processing 21840 -DCPD1MS 0.25 -UW4 preparation method, comprising the following steps:

[0078] (1) Preparation of dihydrate calcium hydrogen phosphate suspension DCPD1-UW4: According to the mass ratio of dihydrate calcium hydrogen phosphate to ultrapure water being 1:4, the weighed dihydrate calcium hydrogen phosphate and ultrapure water were stirred and mixed uniformly at room temperature to prepare dihydrate calcium hydrogen phosphate suspension DCPD1-UW4.

[0079] (2) Corn starch suspension containing dibasic calcium phosphate dihydrate DCPD1MS 0.25 - Preparation of UW4: According to the mass ratio of dihydrate calcium phosphate to corn starch of 1:0.25, the weighed corn starch is added to the dihydrate calcium phosphate suspension of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss.

[0080] (3) Calcium hydrogen phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT 21840 -DCPD1MS 0.25 Preparation of -UW4: The corn starch suspension containing dihydrogen calcium phosphate dihydrate prepared in step (2) is placed in a microwave reactor for treatment, and the energy value obtained per gram of corn starch is controlled to be 21840J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1min and stirred for 10s until the microwave is finished. Then, the prepared pregelatinized corn starch system containing dihydrogen calcium phosphate dihydrate is freeze-dried to obtain a dihydrogen calcium phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT 21840 -DCPD1MS 0.25 -UW4.

[0081] Example 13

[0082] A pregelatinized auxiliary material MT of calcium hydrogen phosphate dihydrate and corn starch co-processing 1310 -The preparation method of DCPD1MS1-UW8 comprises the following steps:

[0083] (1) Preparation of dihydrate calcium hydrogen phosphate suspension DCPD1-UW8: According to the mass ratio of dihydrate calcium hydrogen phosphate to ultrapure water being 1:8, the weighed dihydrate calcium hydrogen phosphate and ultrapure water were stirred and mixed uniformly at room temperature to prepare dihydrate calcium hydrogen phosphate suspension DCPD1-UW8.

[0084] (2) Preparation of corn starch suspension DCPD1MS1-UW8 containing dibasic calcium phosphate dihydrate: According to the mass ratio of dibasic calcium phosphate dihydrate to corn starch of 1:1, the weighed corn starch is added to the dibasic calcium phosphate dihydrate suspension of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss.

[0085] (3) Calcium hydrogen phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT 1310 Preparation of -DCPD1MS1-UW8: The corn starch suspension containing dihydrogen calcium phosphate dihydrate prepared in step (2) is placed in a microwave reactor for treatment, and the energy value obtained per gram of corn starch is controlled to be 1310J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1min and stirred for 10s until the microwave is finished. Then, the prepared pregelatinized corn starch system containing dihydrogen calcium phosphate dihydrate is freeze-dried to obtain a dihydrogen calcium phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT 1310 -DCPD1MS1-UW8.

[0086] Embodiment 14

[0087] A pregelatinized auxiliary material MT of calcium hydrogen phosphate dihydrate and corn starch co-processing 21840-The preparation method of DCPD1MS1-UW8 comprises the following steps:

[0088] (1) Preparation of dihydrate calcium hydrogen phosphate suspension DCPD1-UW8: According to the mass ratio of dihydrate calcium hydrogen phosphate to ultrapure water being 1:8, the weighed dihydrate calcium hydrogen phosphate and ultrapure water were stirred and mixed uniformly at room temperature to prepare dihydrate calcium hydrogen phosphate suspension DCPD1-UW8.

[0089] (2) Preparation of corn starch suspension DCPD1MS1-UW8 containing dibasic calcium phosphate dihydrate: According to the mass ratio of dibasic calcium phosphate dihydrate to corn starch of 1:1, the weighed corn starch is added to the dibasic calcium phosphate dihydrate suspension of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss.

[0090] (3) Calcium hydrogen phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT 21840 Preparation of -DCPD1MS1-UW8: The corn starch suspension containing dihydrogen calcium phosphate dihydrate prepared in step (2) is placed in a microwave reactor for treatment, and the energy value obtained per gram of corn starch is controlled to be 21840J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1min and stirred for 10s until the microwave is finished. Then, the prepared pregelatinized corn starch system containing dihydrogen calcium phosphate dihydrate is freeze-dried to obtain a dihydrogen calcium phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT 21840 -DCPD1MS1-UW8.

[0091] Embodiment 15

[0092] A pregelatinized auxiliary material MT of calcium hydrogen phosphate dihydrate and corn starch co-processing 1310 -DCPD1MS 0.25 -UW8 preparation method, comprising the following steps:

[0093] (1) Preparation of dihydrate calcium hydrogen phosphate suspension DCPD1-UW8: According to the mass ratio of dihydrate calcium hydrogen phosphate to ultrapure water being 1:8, the weighed dihydrate calcium hydrogen phosphate and ultrapure water were stirred and mixed uniformly at room temperature to prepare dihydrate calcium hydrogen phosphate suspension DCPD1-UW8.

[0094] (2) Corn starch suspension containing dibasic calcium phosphate dihydrate DCPD1MS 0.25 - Preparation of UW8: According to the mass ratio of dihydrate calcium phosphate to corn starch of 1:0.25, the weighed corn starch is added to the dihydrate calcium phosphate suspension of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss.

[0095] (3) Calcium hydrogen phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT1310 -DCPD1MS 0.25 Preparation of -UW8: The corn starch suspension containing dihydrogen calcium phosphate dihydrate prepared in step (2) is placed in a microwave reactor for treatment, and the energy value obtained per gram of corn starch is controlled to be 1310J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1min and stirred for 10s until the microwave is finished. Then, the prepared pregelatinized corn starch system containing dihydrogen calcium phosphate dihydrate is freeze-dried to obtain a dihydrogen calcium phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT 1310 -DCPD1MS 0.25 -UW8.

[0096] Example 16

[0097] A pregelatinized auxiliary material MT of calcium hydrogen phosphate dihydrate and corn starch co-processing 21840 -DCPD1MS 0.25 -UW8 preparation method, comprising the following steps:

[0098] (1) Preparation of dihydrate calcium hydrogen phosphate suspension DCPD1-UW8: According to the mass ratio of dihydrate calcium hydrogen phosphate to ultrapure water being 1:8, the weighed dihydrate calcium hydrogen phosphate and ultrapure water were stirred and mixed uniformly at room temperature to prepare dihydrate calcium hydrogen phosphate suspension DCPD1-UW8.

[0099] (2) Corn starch suspension containing dibasic calcium phosphate dihydrate DCPD1MS 0.25 - Preparation of UW8: According to the mass ratio of dihydrate calcium phosphate to corn starch of 1:0.25, the weighed corn starch is added to the dihydrate calcium phosphate suspension of step (1), stirred and mixed evenly at room temperature, and sealed with plastic wrap to prevent water loss.

[0100] (3) Calcium hydrogen phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT 21840 -DCPD1MS 0.25 Preparation of -UW8: The corn starch suspension containing dihydrogen calcium phosphate dihydrate prepared in step (2) is placed in a microwave reactor for treatment, and the energy value obtained per gram of corn starch is controlled to be 21840J. In order to make the corn starch microwave pregelatinized uniformly, an intermittent microwave method is used, that is, each microwave treatment is 1min and stirred for 10s until the microwave is finished. Then, the prepared pregelatinized corn starch system containing dihydrogen calcium phosphate dihydrate is freeze-dried to obtain a dihydrogen calcium phosphate dihydrate-corn starch co-processed pregelatinized auxiliary material MT 21840 -DCPD1MS 0.25 -UW8.

[0101] Referring to the preparation method of sodium carbonate-corn starch co-treated pregelatinized auxiliary material, sodium carbonate-wheat starch / potato starch co-treated pregelatinized auxiliary material was prepared. Referring to the preparation method of dibasic calcium phosphate dihydrate-corn starch co-treated pregelatinized auxiliary material, dibasic calcium phosphate dihydrate-wheat starch / potato starch co-treated pregelatinized auxiliary material, tricalcium phosphate-corn starch / wheat starch / potato starch co-treated pregelatinized auxiliary material, calcium carbonate-corn starch / wheat starch / potato starch co-treated pregelatinized auxiliary material, calcium sulfate dihydrate-corn starch / wheat starch / potato starch co-treated pregelatinized auxiliary material and silicon dioxide-corn starch / wheat starch / potato starch co-treated pregelatinized auxiliary material were prepared. The preparation parameters of each co-treated pregelatinized auxiliary material are summarized in Table 1.

[0102] Table 1 Summary of preparation parameters of each co-processed pregelatinized excipient

[0103]

[0104]

[0105]

[0106]

[0107]

[0108]

[0109] For the samples MT of Examples 1 and 2 above 1310 -SC1MS1-UW4, MT 21840 -SC1MS1-UW4 was used for scanning electron microscopy (SEM) to detect the particle size distribution and powder properties of the samples of Examples 1-144. The results are shown in Figure 1 , the method is as follows:

[0110] 1. Instruments: SU-8100 scanning electron microscope from Hitachi, Japan; BT-2006 laser particle size distribution analyzer from Dandong Better; GJ03-09 powder comprehensive characteristics tester from Jiujiu, Baishan.

[0111] 2. SEM detection conditions: 2 kV acceleration voltage, 500 times magnification.

[0112] 3. Powder properties testing items:

[0113] (1) Bulk density (ρ 松): Fixed volume method. Place the sample on top of the vibrating screen and turn on the vibrating screen. Under the action of vibration, the sample passes through the built-in screen and fills the measuring cylinder with a fixed volume of 25ml. Scrape off the excess powder, weigh the total weight of the powder and the container, and deduct the weight of the container to get the weight of the loose powder (M 松 ), in triplicate.

[0114] ρ 松 =M 松 / 25

[0115] (2) Tap density (ρ 振 ): Fixed mass method. Weigh about 10.0g (M 振 ) sample, put it into a 25ml measuring cylinder, set the speed to 300r / min, and vibrate for 10min. After the vibration is over, read and record the volume of the sample in the measuring cylinder as the vibrated volume (V 振 ).

[0116] ρ 振 =M 振 / V 振

[0117] (3) Carr Index and Hausner Ratio

[0118] The compressibility of powders by the Carr index reaction and the flowability of powders by the Hausner ratio reaction can be calculated by the following formulas, respectively.

[0119] Carr index = (ρ 振 -ρ 松 ) / ρ 振

[0120] Hausner ratio = ρ 振 / ρ 松

[0121] It is not difficult to find that Figure 1 In the SEM test results, MT 1310 -SC1MS1-UW4 corn starch granules swelled after absorbing water, and their volume increased significantly. Their surface was uneven but still spherical, and a small amount of sodium carbonate crystal flocs were adsorbed on the surface. 21840 -SC1MS1-UW4 As the energy value imparted by microwaves to corn starch increases, some starch granules begin to lose their spherical shape and break into irregular fragments, with a large amount of sodium carbonate crystal flocs adsorbed on the surface of the fragments.

[0122] Table 2 Particle size distribution

[0123]

[0124]

[0125]

[0126]

[0127]

[0128]

[0129] As shown in the particle size distribution table of Table 2, the Dv10, Dv50 and Dv90 values ​​represent the particle sizes when the cumulative percentage of particles is 10%, 50% and 90%, respectively. The Dv10, Dv50 and Dv90 values ​​of Examples 1-144 all show a trend of gradually increasing with the increase of the energy value of the microwave imparted to the starch, that is, the degree of swelling, breaking and reunion of the starch particles gradually deepens. At the same time, the mass ratio of the medicinal inorganic salt and / or medicinal inorganic oxide, water and starch will also have a certain influence on the particle size of the co-processed excipients, but the influence of the microwave energy value on the particle size is more obvious.

[0130] Table 3 Powder properties data table

[0131]

[0132]

[0133]

[0134]

[0135]

[0136]

[0137] As shown in Table 3, the powder properties of the samples prepared in Examples 1-144 show a decreasing trend in angle of repose, Hausner ratio, and Carr index as the energy value of the microwave imparted to the starch increases, that is, the fluidity and compressibility of the powder show an increasing trend. At the same time, the mass ratio of the medicinal inorganic salt and / or medicinal inorganic oxide, water, and starch will also have a certain influence on the powder properties of the co-processed excipients, but the microwave energy value has a more obvious influence on it, which is consistent with the conclusion of the above particle size.

[0138] Compression of blank effervescent tablets based on the sodium carbonate-starch co-processed pregelatinized excipients prepared in Examples 1-8 and Examples 17-32.

[0139] The sodium carbonate-starch co-processed pregelatinized excipients of Examples 1-8 and Examples 17-32 were tableted according to the prescription in Table 4, and the relevant inspection indicators are shown in the table.

[0140] Compression of blank tablets based on the inorganic compound-starch co-processed pregelatinized excipients of Examples 9-16 and Examples 33-144.

[0141] The inorganic compound-starch co-processed pregelatinized excipients of Examples 9-16 and Examples 33-144 were tableted according to the prescription in Table 5. The relevant inspection indicators are shown in the table.

[0142] Table 4 Blank effervescent tablet prescription design

[0143]

[0144]

[0145] Table 5 Blank tablet prescription design

[0146] Excipient name Proportion(%) Co-processing of pre-gelatinized excipients 100

[0147] The powder direct tableting method was adopted for preparation: the co-processed pregelatinized excipients of Examples 1-8 and Examples 17-32 were weighed as the basic excipients of the blank effervescent tablets according to the prescription amount in Table 4, and the powder was directly compressed according to the tablet weight of 350 mg, the tablet diameter of 12.0 mm, the tablet thickness of 3.5 mm, and the hardness of 8 to 10 kg. The co-processed pregelatinized excipients of Examples 9-16 and Examples 33-144 were weighed as the basic excipients of the blank tablets according to the prescription amount in Table 5, and the powder was directly compressed according to the tablet weight of 350 mg, the tablet diameter of 12.0 mm, the tablet thickness of 3.5 mm, and the hardness of 8 to 10 kg.

[0148] Determination of disintegration time: One tablet of each tablet prepared according to the above prescription was tested for disintegration time according to the disintegration time determination method for ordinary tablets in Part 4 of the Chinese Pharmacopoeia.

[0149] Table 6 Disintegration time of tablets

[0150]

[0151]

[0152]

[0153]

[0154]

[0155]

[0156] It can be seen that as the energy value imparted by microwaves to starch increases, the disintegration time of the compressed tablets is extended. Therefore, manufacturers can control the degree of starch pregelatinization by changing microwave energy parameters to meet the disintegration time requirements of different tablets. This may have certain application value in oral solid sustained-release preparations and orodisintegrating tablets.

[0157] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

Claims

1. A method for preparing an inorganic compound-starch co-processed pregelatinized auxiliary material, characterized in that: The preparation method comprises: Mixing the medicinal inorganic salt and / or medicinal inorganic oxide with water and then mixing with starch; placing the mixed system in a microwave reactor for microwave treatment; The microwaved product was dried.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the medicinal inorganic salt and / or medicinal inorganic oxide, water and starch is 1:4-16:0.25-5.

3. The preparation method according to claim 1, characterized in that: The pharmaceutical inorganic salt is selected from sodium carbonate, calcium carbonate, calcium hydrogen phosphate dihydrate, tricalcium phosphate or calcium sulfate dihydrate.

4. The preparation method according to claim 1, characterized in that: The medicinal inorganic oxide is silicon dioxide.

5. The preparation method according to claim 1, characterized in that: The starch is selected from corn starch, potato starch or wheat starch.

6. The preparation method according to claim 1, characterized in that: In the microwave treatment, the time and frequency of the microwave treatment are adjusted so that the microwave energy value obtained per gram of starch is 1310J to 21840J.

7. The inorganic compound-starch co-processed pregelatinized auxiliary material prepared according to the method of any one of claims 1 to 6.

8. A pharmaceutical preparation, characterized in that It contains the inorganic compound-starch co-processed pregelatinized auxiliary material as claimed in claim 7.

9. Use of the inorganic compound-starch co-processed pregelatinized auxiliary material according to claim 7 in dry or wet granulation.

10. Use of the inorganic compound-starch co-processed pregelatinized auxiliary material according to claim 7 in direct powder tableting.

Citation Information

Patent Citations

  • Method for producing high-flowability pregelatinized starch

    CN102134281A

  • Starch-based hydrogel carrier material for controlling slow-release, and preparation method and application thereof

    CN102824643A

  • Method for preparing medicinal premixed ingredients

    CN103127517A

  • Preparation method of medicinal pregelatinized starch

    CN104193834A

  • Direct compression composite accessory and preparation method thereof

    CN104548112A

Cited By

  • Pre-gelatinized starch / calcium-containing mineral-berberine compound as well as preparation method and application thereof

    CN120586075A