Recyclable filter aid for filtering fluorine-containing sludge pickling reaction liquid and preparation method thereof
Through the core-shell magnetic nanoparticle filter aid modified by alkyl carboxylic acid, the problems of low separation efficiency and secondary pollution of calcium fluoride during the pickling process are solved, and efficient filtration and dehydration and stable recycling are achieved, which significantly improves the The purification effect of calcium fluoride.
Patent Information
- Application Number
- CN202411193932.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art is difficult to efficiently separate calcium fluoride in fluorine-containing sludge during the pickling process, and common filter aids are prone to residues, resulting in secondary contamination and difficulty in recycling.
Core-shell magnetic nanoparticles modified with alkyl carboxylic acid are prepared by co-precipitation, coating, surface modification and alkyl carboxylic acid modification treatment to form stable magnetic nanoparticles for enhanced filtration separation Efficiency and recycling.
The filtering and dehydration efficiency is significantly improved, the filtration time is shortened, the moisture content of the filter cake is reduced, and the filter aid is easy to separate magnets, with good recycling performance, and avoiding secondary contamination of calcium fluoride products.
Smart Images

Figure BDA0005015818060000071
Abstract
Description
Technical Field
[0001] The invention relates to a filtering and dehydrating process for purifying calcium fluoride products in fluoride-containing sludge by an acid treatment method, and in particular to a recyclable filter aid for filtering and dehydrating fluoride-containing sludge acid washing reaction liquid and a preparation method thereof. Background Art
[0002] As the main source of environmental fluoride pollution, fluoride-containing wastewater has the characteristics of wide sources, high content and great harm. Its treatment is an important part of preventing and controlling fluoride pollution. At present, the basic idea of fluoride removal from industrial fluoride-containing wastewater is to transfer the fluorine element from the liquid phase to the solid phase. The main methods include calcium salt precipitation method, coagulation precipitation method and physical adsorption method. With the gradual increase in the volume and treatment scale of fluoride-containing wastewater, the output of fluoride-containing sludge has also increased year by year. The chemical composition of fluoride-containing sludge is mainly calcium fluoride, and also includes impurities such as calcium carbonate, calcium hydroxide, calcium sulfate, calcium silicate and flocculants. Among them, calcium fluoride is an important upstream raw material of the fluorine chemical industry. Therefore, it is of great significance to extract and separate calcium fluoride from fluoride-containing sludge.
[0003] The main impurity components of fluoride-containing sludge can react chemically with medium-strong acids and dissolve in acid solutions, while calcium fluoride is basically insoluble in other medium-strong acids except for reacting with concentrated sulfuric acid. Therefore, most of the impurities in fluoride-containing sludge can be removed through the pickling process, and the calcium fluoride content in the remaining solids can be significantly increased. Since silica colloids are produced during the acid treatment process, the colloids and the flocculants in the sludge are highly hydrophilic, making it difficult to separate the pickling liquid and the remaining solids by filtration. In most difficult-to-filter systems, the use of filter aids to enhance filtration is considered to be one of the feasible solutions. However, ordinary physical filter aids and chemical filter aids are easily left in the filter cake and filtrate, respectively, which on the one hand causes secondary pollution of the calcium fluoride product, and on the other hand has a negative impact on the treatment effect of the recycled pickling liquid. Therefore, constructing a highly efficient filter aid that is easy to separate from the filter cake filtrate and can be recycled is one of the important technical difficulties in solid-liquid separation after calcium fluoride pickling. Summary of the invention
[0004] The present invention provides a filter aid for dehydrating fluorine-containing sludge pickling reaction liquid and a preparation method thereof, so as to simultaneously solve the technical problems of strengthening filtration separation, avoiding secondary pollution, and facilitating recycling and reuse, and realize efficient separation of solid products in the pickling reaction liquid and the pickling liquid.
[0005] In order to solve the above problems, the present invention discloses a recyclable filter aid for filtering and dehydrating fluorine-containing sludge pickling reaction liquid, characterized in that the main component is core-shell magnetic nanoparticles modified with alkyl carboxylic acid.
[0006] A method for preparing a recyclable filter aid for filtering and dehydrating a fluorine-containing sludge pickling reaction liquid, comprising the following steps:
[0007] (1) Preparation of magnetic ferroferric oxide nanoparticles by coprecipitation method
[0008] Weigh 3.89g of ferric chloride and 3.34g of ferrous sulfate heptahydrate and dissolve them in 400mL of deionized water, start stirring, heat to 50°C at 300rpm, add 30mL of 15% sodium hydroxide solution under nitrogen protection, continue crystallization for 1 hour after the addition, separate the solid product by magnet, and dry it in an oven at 120°C for 2 hours to obtain magnetic ferrosoferric oxide nanoparticles;
[0009] (2) Preparation of Silica-coated Magnetic FeO4 Nanoparticles
[0010] Weigh 2 g of the magnetic ferroferric oxide nanoparticles obtained in step (1), and uniformly disperse them into 200 mL of a mixture of ethanol and water (v / v=4 / 1) by ultrasound. Add 2 mL of 25% ammonia water under stirring at 30° C. and 300 rpm, then add ethyl orthosilicate to the mixed solution, continue stirring and reacting for 10 hours, separate the solid product by a magnet, and dry it in an oven at 120° C. for 2 hours to obtain core-shell Fe3O4@SiO2 magnetic nanoparticles (hereinafter referred to as core-shell magnetic nanoparticles).
[0011] (3) Surface amino modification of core-shell magnetic nanoparticles
[0012] Weigh 2 g of the core-shell magnetic nanoparticles prepared in step (2), and evenly disperse them in 200 mL of ethanol by ultrasound. Then, add 3-aminopropyltriethoxysilane under mechanical stirring, react at 30° C. for 12 hours, separate the solid product with a magnet, wash with anhydrous ethanol to remove unreacted 3-aminopropyltriethoxysilane, and dry in an oven at 120° C. for 2 hours to obtain amino-terminated functionalized core-shell magnetic nanoparticles (hereinafter referred to as amino-terminated core-shell magnetic particles);
[0013] (4) Alkyl carboxylic acid modification of core-shell magnetic particles
[0014] Weigh 1 g of the amino-modified core-shell magnetic particles obtained in step (3), and uniformly disperse them in 100 mL of organic solvent DMF by ultrasound. Then, add alkyl dicarboxylic acid and catalyst under mechanical stirring, and react at 120° C. for 24 hours. Wash the solid product collected by a magnet with anhydrous ethanol, and dry it in an oven at 120° C. for 2 hours to obtain alkyl carboxylic acid-modified core-shell magnetic particles.
[0015] In step 2 of the above method, the amount of ethyl orthosilicate used is 2 to 5 mL.
[0016] In step 2 of the above method, the ethyl orthosilicate is added dropwise into the reaction solution through a dropping funnel at a rate of 1 to 2 drops per second.
[0017] In step 3 of the above method, the amount of 3-aminopropyltriethoxysilane used is 0.5 to 1 g.
[0018] In step 4 of the above method, the alkyl dicarboxylic acid is one of alkyl dicarboxylic acids with different hydrocarbon chain lengths, specifically one of sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid and octadecanedioic acid.
[0019] In step 4 of the above method, the amount of the alkyl dicarboxylic acid used is 0.2 to 1 g.
[0020] In step 4 of the above method, the catalyst is 4-dimethylaminopyridine, and its usage is 0.02-0.1 g.
[0021] The present invention has the following advantages:
[0022] (1) The present invention coats the surface of magnetic ferroferric oxide nanoparticles with silicon dioxide, so that the magnetic carrier can stably exist in a strong acidic environment. The multi-hydroxyl groups on the surface of the core-shell magnetic particles are very beneficial for anchoring alkyl carboxylic acid surfactants. The alkyl carboxylic acid surfactants are immobilized on the core-shell magnetic particles through chemical covalent bonds, and the preparation method is simple.
[0023] (2) The alkyl carboxylic acid modified core-shell magnetic particles prepared by the present invention can significantly improve the filtration and dehydration efficiency in the process of acid washing and impurity removal of fluorine-containing sludge, significantly shorten the filtration time, and significantly reduce the moisture content of the sludge filter cake. In addition, the magnetic filter aid is easy to separate from the fluorine-containing sludge by magnets, and has stable recycling performance, and has a good application prospect. DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0025] Example 1
[0026] Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring and heat to 50° C. at 300 rpm. Add 30 mL of 15% sodium hydroxide solution under nitrogen protection. After the addition, continue crystallization for 1 hour. Separate the solid product by a magnet and dry it in an oven at 120° C. for 2 hours to obtain magnetic ferrosoferric oxide nanoparticles.
[0027] Weigh 2 g of the above-mentioned magnetic ferroferric oxide nanoparticles, uniformly disperse them into 200 mL of a mixture of ethanol and water (v / v=4 / 1) by ultrasound, add 2 mL of 25% ammonia water under stirring at 30°C and 300 rpm, then add 3 mL of ethyl orthosilicate dropwise into the above-mentioned mixed solution, continue stirring and react for 10 hours, separate the solid product by a magnet, and dry it in an oven at 120°C for 2 hours to obtain core-shell Fe3O4@SiO2 magnetic nanoparticles (hereinafter referred to as core-shell magnetic nanoparticles).
[0028] Weigh 2 g of the above core-shell magnetic nanoparticles, uniformly disperse them in 200 mL of ethanol by ultrasound, then add 1 g of 3-aminopropyltriethoxysilane under mechanical stirring, react at 30° C. for 12 hours, separate the solid product with a magnet, wash with anhydrous ethanol to remove unreacted 3-aminopropyltriethoxysilane, and dry in an oven at 120° C. for 2 hours to obtain amino-terminated functionalized core-shell magnetic nanoparticles (hereinafter referred to as amino-terminated core-shell magnetic particles).
[0029] Weigh 1 g of the above-mentioned aminated core-shell magnetic particles and uniformly disperse them in 100 mL of organic solvent DMF by ultrasound. Then, 0.6 g of sebacic acid and 0.05 g of catalyst 4-dimethylaminopyridine are added under mechanical stirring, and the mixture is reacted at 120° C. for 24 hours. The solid product collected by the magnet is washed with anhydrous ethanol and dried in an oven at 120° C. for 2 hours to obtain alkyl carboxylic acid-modified core-shell magnetic particles.
[0030] Example 2
[0031] Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring and heat to 50° C. at 300 rpm. Add 30 mL of 15% sodium hydroxide solution under nitrogen protection. After the addition, continue crystallization for 1 hour. Separate the solid product by a magnet and dry it in an oven at 120° C. for 2 hours to obtain magnetic ferrosoferric oxide nanoparticles.
[0032] Weigh 2 g of the above-mentioned magnetic ferroferric oxide nanoparticles, uniformly disperse them into 200 mL of a mixture of ethanol and water (v / v=4 / 1) by ultrasound, add 2 mL of 25% ammonia water under stirring at 30°C and 300 rpm, then add 3 mL of ethyl orthosilicate dropwise into the above-mentioned mixed solution, continue stirring and react for 10 hours, separate the solid product by a magnet, and dry it in an oven at 120°C for 2 hours to obtain core-shell Fe3O4@SiO2 magnetic nanoparticles (hereinafter referred to as core-shell magnetic nanoparticles).
[0033] Weigh 2 g of the above core-shell magnetic nanoparticles, uniformly disperse them in 200 mL of ethanol by ultrasound, then add 1 g of 3-aminopropyltriethoxysilane under mechanical stirring, react at 30° C. for 12 hours, separate the solid product with a magnet, wash with anhydrous ethanol to remove unreacted 3-aminopropyltriethoxysilane, and dry in an oven at 120° C. for 2 hours to obtain amino-terminated functionalized core-shell magnetic nanoparticles (hereinafter referred to as amino-terminated core-shell magnetic particles).
[0034] 1 g of the above-mentioned aminated core-shell magnetic particles were weighed and uniformly dispersed in 100 mL of organic solvent DMF by ultrasound, and then 0.6 g of dodecyl dicarboxylic acid and 0.05 g of catalyst 4-dimethylaminopyridine were added under mechanical stirring, and the mixture was reacted at 120° C. for 24 hours. The solid product collected by the magnet was washed with anhydrous ethanol and dried in an oven at 120° C. for 2 hours to obtain alkyl carboxylic acid-modified core-shell magnetic particles.
[0035] Example 3
[0036] Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring and heat to 50° C. at 300 rpm. Add 30 mL of 15% sodium hydroxide solution under nitrogen protection. After the addition, continue crystallization for 1 hour. Separate the solid product by a magnet and dry it in an oven at 120° C. for 2 hours to obtain magnetic ferrosoferric oxide nanoparticles.
[0037] Weigh 2 g of the above-mentioned magnetic ferroferric oxide nanoparticles, uniformly disperse them into 200 mL of a mixture of ethanol and water (v / v=4 / 1) by ultrasound, add 2 mL of 25% ammonia water under stirring at 30°C and 300 rpm, then add 3 mL of ethyl orthosilicate dropwise into the above-mentioned mixed solution, continue stirring and react for 10 hours, separate the solid product by a magnet, and dry it in an oven at 120°C for 2 hours to obtain core-shell Fe3O4@SiO2 magnetic nanoparticles (hereinafter referred to as core-shell magnetic nanoparticles).
[0038] Weigh 2 g of the above core-shell magnetic nanoparticles, uniformly disperse them in 200 mL of ethanol by ultrasound, then add 1 g of 3-aminopropyltriethoxysilane under mechanical stirring, react at 30° C. for 12 hours, separate the solid product with a magnet, wash with anhydrous ethanol to remove unreacted 3-aminopropyltriethoxysilane, and dry in an oven at 120° C. for 2 hours to obtain amino-terminated functionalized core-shell magnetic nanoparticles (hereinafter referred to as amino-terminated core-shell magnetic particles).
[0039] 1 g of the above-mentioned aminated core-shell magnetic particles were weighed and uniformly dispersed in 100 mL of organic solvent DMF by ultrasound, and then 0.6 g of tetradecyl dicarboxylic acid and 0.05 g of catalyst 4-dimethylaminopyridine were added under mechanical stirring, and the mixture was reacted at 120° C. for 24 hours. The solid product collected by the magnet was washed with anhydrous ethanol and dried in an oven at 120° C. for 2 hours to obtain alkyl carboxylic acid-modified core-shell magnetic particles.
[0040] Example 4
[0041] Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring and heat to 50° C. at 300 rpm. Add 30 mL of 15% sodium hydroxide solution under nitrogen protection. After the addition, continue crystallization for 1 hour. Separate the solid product by a magnet and dry it in an oven at 120° C. for 2 hours to obtain magnetic ferrosoferric oxide nanoparticles.
[0042] Weigh 2 g of the above-mentioned magnetic ferroferric oxide nanoparticles, uniformly disperse them into 200 mL of a mixture of ethanol and water (v / v=4 / 1) by ultrasound, add 2 mL of 25% ammonia water under stirring at 30°C and 300 rpm, then add 3 mL of ethyl orthosilicate dropwise into the above-mentioned mixed solution, continue stirring and react for 10 hours, separate the solid product by a magnet, and dry it in an oven at 120°C for 2 hours to obtain core-shell Fe3O4@SiO2 magnetic nanoparticles (hereinafter referred to as core-shell magnetic nanoparticles).
[0043] Weigh 2 g of the above core-shell magnetic nanoparticles, uniformly disperse them in 200 mL of ethanol by ultrasound, then add 1 g of 3-aminopropyltriethoxysilane under mechanical stirring, react at 30° C. for 12 hours, separate the solid product with a magnet, wash with anhydrous ethanol to remove unreacted 3-aminopropyltriethoxysilane, and dry in an oven at 120° C. for 2 hours to obtain amino-terminated functionalized core-shell magnetic nanoparticles (hereinafter referred to as amino-terminated core-shell magnetic particles).
[0044] 1 g of the above-mentioned aminated core-shell magnetic particles were weighed and uniformly dispersed in 100 mL of organic solvent DMF by ultrasound, and then 0.6 g of hexadecyl dicarboxylic acid and 0.05 g of catalyst 4-dimethylaminopyridine were added under mechanical stirring, and the mixture was reacted at 120° C. for 24 hours. The solid product collected by the magnet was washed with anhydrous ethanol and dried in an oven at 120° C. for 2 hours to obtain alkyl carboxylic acid-modified core-shell magnetic particles.
[0045] Example 5
[0046] Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring and heat to 50° C. at 300 rpm. Add 30 mL of 15% sodium hydroxide solution under nitrogen protection. After the addition, continue crystallization for 1 hour. Separate the solid product by a magnet and dry it in an oven at 120° C. for 2 hours to obtain magnetic ferrosoferric oxide nanoparticles.
[0047] Weigh 2 g of the above-mentioned magnetic ferroferric oxide nanoparticles, uniformly disperse them into 200 mL of a mixture of ethanol and water (v / v=4 / 1) by ultrasound, add 2 mL of 25% ammonia water under stirring at 30°C and 300 rpm, then add 3 mL of ethyl orthosilicate dropwise into the above-mentioned mixed solution, continue stirring and react for 10 hours, separate the solid product by a magnet, and dry it in an oven at 120°C for 2 hours to obtain core-shell Fe3O4@SiO2 magnetic nanoparticles (hereinafter referred to as core-shell magnetic nanoparticles).
[0048] Weigh 2 g of the above core-shell magnetic nanoparticles, uniformly disperse them in 200 mL of ethanol by ultrasound, then add 1 g of 3-aminopropyltriethoxysilane under mechanical stirring, react at 30° C. for 12 hours, separate the solid product with a magnet, wash with anhydrous ethanol to remove unreacted 3-aminopropyltriethoxysilane, and dry in an oven at 120° C. for 2 hours to obtain amino-terminated functionalized core-shell magnetic nanoparticles (hereinafter referred to as amino-terminated core-shell magnetic particles).
[0049] 1 g of the above-mentioned aminated core-shell magnetic particles were weighed and uniformly dispersed in 100 mL of organic solvent DMF by ultrasound, and then 0.6 g of octadecyl dicarboxylic acid and 0.05 g of catalyst 4-dimethylaminopyridine were added under mechanical stirring, and the mixture was reacted at 120° C. for 24 hours. The solid product collected by the magnet was washed with anhydrous ethanol and dried in an oven at 120° C. for 2 hours to obtain alkyl carboxylic acid-modified core-shell magnetic particles.
[0050] Application Example 1
[0051] Using fluorine-containing sludge (water content of 55%, calcium fluoride dry content of 60.35%) produced by a certain enterprise in Guangdong as raw material, 1+9 hydrochloric acid as pickling reagent, 750g of fluorine-containing sludge was crushed and added to 500mL of pickling reagent, and the reaction was stirred at room temperature and 300rpm for 4 hours to obtain fluorine-containing sludge pickling reaction liquid. The core-shell magnetic particles modified with alkyl carboxylic acids of Examples 1 to 5 were used as filter aids to conduct a filtration test on the above-mentioned fluorine-containing sludge pickling reaction liquid. The specific steps are as follows: 0.1 to 0.5 g of filter aid was weighed and added to the above-mentioned fluorine-containing sludge pickling reaction liquid, stirred at room temperature and 300 rpm for 5 minutes, and then filtered with a Buchner funnel with a diameter of 11 cm, with a vacuum degree of 0.09 MPa, and filtered until no liquid dripped within 1 minute, and the filtration time and the mass of the wet filter cake were recorded, and then the filter cake was placed in a 120-degree oven to dry to constant weight and the weight of the dry filter cake was recorded, the moisture content of the wet filter cake was calculated, and the calcium fluoride content in the dry filter cake was tested. As a blank application example, the above operation was performed without adding any filter aid. The above test results are shown in Table 1.
[0052] Table 1 Effect of filter aid type and dosage on filtration performance and calcium fluoride content of fluoride-containing sludge pickling reaction liquid
[0053] Test No. Filter aid type Filter aid dosage / g Filter time / s Wet cake moisture content / % Calcium fluoride dry basis content / % 1 blank 0 5230 54.60 73.45 2 Example 1 0.5 2896 44.83 81.56 3 Example 2 0.5 2764 43.27 82.40 4 Example 3 0.5 2659 42.28 83.52 5 Example 4 0.5 2583 41.64 83.85 6 Example 5 0.5 2461 40.78 84.21 7 Example 5 0.1 4725 51.63 76.63 8 Example 5 0.3 3645 47.60 79.37
[0054] As shown in Table 1, compared with the blank filtration test, the filter aids in all examples can significantly shorten the filtration time and reduce the moisture content of the wet filter cake, and the calcium fluoride content in the obtained filter cake is also significantly improved compared with the blank filtration test. In particular, the filter aid in Example 5 has the best filter dehydration and calcium fluoride purification effect.
[0055] Application Example 2
[0056] For application test 6 in application example 1, a recycling test of the filter aid was conducted, and the relevant filtration steps were the same as those described in application example 1. A magnet was used to separate the acid-washed residual solid and the filter aid after drying, and the recovered mass of the filter aid was recorded. The mass of the filter aid was slightly lost, mainly due to adhesion to the vessel wall and filter paper during the filtration process. The recovered filter aid was used to conduct the same application test, and was recycled 3 times according to the above method. The application effect is shown in Table 2.
[0057] Table 2 Effect of the number of cycles on the filtration performance and calcium fluoride content of the filter aid in application test 6 of Example 1
[0058]
[0059] It can be seen from Table 2 that the filter aid of the present invention has the advantages of easy recovery, excellent filtering effect, stable recycling performance, etc. during the recycling process, and the calcium fluoride content in the purified product is also significantly improved compared with the blank filtration test. In summary, the filter aid has good application prospects.
Claims
1. A recyclable filter aid for filtering and dehydrating fluorine-containing sludge pickling reaction liquid, characterized in that: The main component is core-shell magnetic nanoparticles modified with alkyl carboxylic acid.
2. A method for preparing a recyclable filter aid for filtering and dehydrating fluorine-containing sludge pickling reaction liquid as claimed in claim 1, characterized in that: The preparation process includes steps (1) to (4): (1) Preparation of magnetic FeO4 nanoparticles by coprecipitation method Weigh 3.89 g of ferric chloride and 3.34 g of ferrous sulfate heptahydrate and dissolve them in 400 mL of deionized water. Start stirring, heat to 50°C at 300 rpm, add 30 mL of 15% sodium hydroxide solution under nitrogen protection, continue crystallization for 1 hour after the addition, separate the solid product by magnet, and dry it in an oven at 120°C for 2 hours to obtain magnetic ferrosoferric oxide nanoparticles; (2) Preparation of silica-coated magnetic FeO nanoparticles Weigh 2 g of the magnetic ferroferric oxide nanoparticles prepared in step (1), and uniformly disperse them into 200 mL of a mixture of ethanol and water (v / v=4 / 1) by ultrasonication. Add 2 mL of 25% ammonia water under stirring at 30° C. and 300 rpm, then add ethyl orthosilicate to the mixed solution, continue stirring and reacting for 10 hours, separate the solid product by a magnet, and dry it in an oven at 120° C. for 2 hours to obtain core-shell Fe3O4@SiO2 magnetic nanoparticles (hereinafter referred to as core-shell magnetic nanoparticles). (3) Surface amino modification of core-shell magnetic nanoparticles Weigh 2 g of the core-shell magnetic nanoparticles prepared in step (2), and evenly disperse them in 200 mL of ethanol by ultrasonication. Then, add 3-aminopropyltriethoxysilane under mechanical stirring, and react at 30° C. for 12 hours. Separate the solid product with a magnet, wash with anhydrous ethanol to remove unreacted 3-aminopropyltriethoxysilane, and dry in an oven at 120° C. for 2 hours to obtain amino-terminated functionalized core-shell magnetic nanoparticles (hereinafter referred to as amino-terminated core-shell magnetic particles). (4) Alkyl carboxylic acid modification of core-shell magnetic particles Weigh 1 g of the amino-modified core-shell magnetic particles obtained in step (3), and disperse them uniformly in 100 mL of organic solvent DMF by ultrasound. Then, add alkyl dicarboxylic acid and catalyst under mechanical stirring, and react at 120° C. for 24 hours. Wash the solid product collected by magnet with anhydrous ethanol and dry it in an oven at 120° C. for 2 hours to obtain alkyl carboxylic acid-modified core-shell magnetic particles.
3. A method for preparing a recyclable filter aid for filtering and dehydrating fluorine-containing sludge pickling reaction liquid according to claim 2, characterized in that: In the step (2), the amount of tetraethyl orthosilicate used is 2-5 mL.
4. The method for preparing a recyclable filter aid for filtering and dehydrating fluorine-containing sludge pickling reaction liquid according to claim 2, characterized in that: In the step (2), ethyl orthosilicate is added dropwise into the reaction solution through a dropping funnel at a rate of 1 to 2 drops per second.
5. The method for preparing a recyclable filter aid for filtering and dehydrating fluorine-containing sludge pickling reaction liquid according to claim 2, characterized in that: In the step (3), the amount of 3-aminopropyltriethoxysilane used is 0.5-1 g.
6. A method for preparing a recyclable filter aid for filtering and dehydrating fluorine-containing sludge pickling reaction liquid according to claim 2, characterized in that: In the step (4), the alkyl dicarboxylic acid is one of alkyl dicarboxylic acids with different hydrocarbon chain lengths, specifically one of sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid and octadecanedioic acid.
7. The method for preparing a recyclable filter aid for filtering and dehydrating fluorine-containing sludge pickling reaction liquid according to claim 2, characterized in that: In the step (4), the amount of alkyl dicarboxylic acid used is 0.2-1 g.
8. The method for preparing a recyclable filter aid for filtering and dehydrating fluorine-containing sludge pickling reaction liquid according to claim 2, characterized in that: In the step (4), the catalyst is 4-dimethylaminopyridine, and the amount used is 0.02-0.1 g.