The specific surface area and pore volume of biochar are improved by ball mill mechanochemical modification method, and combined with magnetic modification, the problems of solid-liquid separation and adsorption performance of biochar in application are solved, achieving efficient wastewater treatment and material recovery.
Patent Information
- Application Number
- CN202411350067.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-29
AI Technical Summary
During the application process, biochar has problems such as small specific surface area and difficulty in solid-liquid separation, and the introduction of magnetic particles may lead to a degradation of adsorption performance.
The ball mill mechanochemical modification method is used to grind, calcin and ball milling. Combined with magnetic modification, the ball mill mechanochemically modified magnetic biochar is prepared to improve its specific surface area and pore volume, and the powder is realized through magnetic properties. Recycling of biochar.
It significantly improves the adsorption performance of biochar and the recycling rate of magnetic biochar, avoids secondary pollution, and is suitable for methylene blue adsorption in acidic, neutral and strong alkaline environments.
Smart Images

Figure CN119034709A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of straw biomass resource utilization and water treatment, and specifically relates to a ball mill mechanical chemically modified magnetic biochar and a preparation method and application thereof. Background Art
[0002] Biochar, as a carbon material with low price, simple preparation and outstanding physical and chemical properties, has been widely used in the field of environmental remediation. However, biochar has disadvantages such as small specific surface area and difficulty in solid-liquid separation during the application process, which greatly limits the application of biochar.
[0004] After adsorption, if the powdered biochar cannot be separated from the water in time, it may cause secondary pollution of the water body, which greatly limits its practical application. In order to solve the problem of biochar recovery, the most effective strategy is to load transition metals and their oxides on biochar, give it magnetism, and separate magnetic biochar by applying an external magnetic field. However, many studies have found that the introduction of magnetic particles may cause the pores of biochar to be blocked, resulting in a decrease in the specific surface area of biochar, thereby causing a decrease in adsorption performance.
[0005] In order to improve the adsorption performance of biochar, certain means are usually used to modify it: common modification methods include acid-base treatment, surfactant modification, ball milling mechanochemical method and other modification methods. Summary of the invention
[0006] In order to solve one of the above problems, the present invention provides a ball milling mechanochemically modified magnetic biochar and a preparation method and application thereof.
[0007] In order to achieve the above object, the present invention adopts the following technical means:
[0008] The first aspect of the present invention provides a method for ball milling mechanochemical modification of magnetic biochar, comprising the following steps:
[0009] (1) The biomass raw material is processed by a crusher, sieved, then fully washed with deionized water, and placed in a drying oven to completely dry;
[0010] (2) placing the biomass raw material powder and potassium trioxalatoferrate in a mortar at a mass ratio of 4:(1-3) and grinding them thoroughly;
[0011] (3) placing the ground mixture in a muffle furnace and calcining it to obtain magnetic biochar;
[0012] (4) The magnetic biochar is ball-milled to obtain the final product, ball-milled magnetic biochar.
[0013] In some embodiments of the present invention, preferably, the biomass raw material is wheat straw.
[0014] In some embodiments of the present invention, the calcination temperature is 500-600° C. and the calcination time is 2-3 h.
[0015] In some embodiments of the present invention, the ball milling conditions are: rotation speed 400-500r / min, processing time 1-2h.
[0016] In some embodiments of the present invention, the mass ratio of magnetic biochar to ball milling beads in the ball mill is 1:(15-25).
[0017] In some embodiments of the present invention, the drying oven is a forced air drying oven, the forced air drying oven temperature is 50-60° C., and the drying time is 8-12 hours.
[0018] The second aspect of the present invention provides a magnetic biochar, which is prepared by the method described in the first aspect.
[0019] The third aspect of the present invention provides the use of magnetic biochar prepared by the method described in the first aspect in adsorbing organic dye wastewater.
[0020] In some embodiments of the present invention, the magnetic biochar is placed in wastewater containing organic dyes, and the pH value of the wastewater containing organic dyes is 3-12.
[0021] In some embodiments of the present invention, the adsorbed magnetic biochar is recovered by magnetic absorption and then washed multiple times with anhydrous ethanol and 0.01 mol / L dilute hydrochloric acid solution before being reused.
[0022] Beneficial effects of the present invention
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) Provide a method for preparing ball-milled mechanochemically modified magnetic biochar, wherein wheat straw is used as raw material for pyrolysis to prepare biochar, and through a step-by-step optimization strategy, the biochar with the best adsorption effect is screened out and the ball milling parameters are determined, and then based on these parameters, a ball-milled mechanochemically modified magnetic biochar is prepared by combining magnetic modification with ball milling chemical modification, which not only realizes the comprehensive utilization of straw, but also solves the water pollution problem.
[0025] (2) Through the characterization and analysis of the physical and chemical properties of the sample materials, it can be seen that: compared with pure biochar, the specific surface area and pore volume of the ball-milled mechanically chemically modified magnetic biochar are increased, and its saturation magnetization intensity is 15.30emu / g. It has strong paramagnetism, which is conducive to the recovery, regeneration and utilization of the powdered biochar after adsorption, avoiding the secondary pollution caused by it.
[0026] (3) In this study, the ball-milled modified magnetic biochar was prepared by magnetic modification followed by ball milling, which had better adsorption performance than conventional ball-milled biochar. The raw materials are easily obtained and the preparation method is simple. It has great application prospects while co-processing waste biomass materials. The ball-milled modified magnetic biochar in this application is suitable for the adsorption of methylene blue in acidic, neutral and alkaline environments, and can even maintain good methylene blue adsorption performance under strong alkaline printing and dyeing wastewater environment conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The XRD patterns of three kinds of biochar obtained in Example 1 of the present invention are shown, wherein BC1 is wheat straw biochar, BC2 is rape straw biochar, and BC3 is corn straw biochar;
[0028] Figure 2 A comparison diagram of the adsorption effects of three types of biochar obtained in Example 1 of the present invention on methylene blue is shown;
[0029] Figure 3 A comparison diagram showing the adsorption effect of three kinds of ball-milled biochars of wheat straw on methylene blue in Example 2 of the present invention is shown;
[0030] Figure 4 The biochar BC, BM-BC1, BM-Fe3O4 / γ-Fe2O in Examples 1 to 3 of the present invention are shown. 3- SEM image of BC1 subjected to electron scanning;
[0031] Figure 5 The biochar BC, BM-BC1, BM-Fe3O4 / γ-Fe2O in Examples 1 to 3 of the present invention are shown. 3- XRD characterization of BC1;
[0032] Figure 6 A comparison diagram of methylene blue adsorption by ball-milled magnetic biochar prepared in Examples 3 to 5 of the present invention is shown;
[0033] Figure 7 A comparison diagram of methylene blue adsorption under different solution initial concentration conditions is shown for ball-milled magnetic biochar prepared in Examples 3 to 5 of the present invention;
[0034] Figure 8 A comparison diagram of the adsorption of methylene blue under different solution pH conditions is shown for the ball-milled magnetic biochar prepared in Example 3 of the present invention;
[0035] Fig. 9 The adsorption of methylene blue by the ball-milled magnetic biochar prepared in Example 3 of the present invention changes with time;
[0036] Fig.10 The hysteresis loop diagram of the ball-milled magnetic biochar prepared in Example 3 of the present invention is shown;
[0037] Fig.11 The figure shows the repeated absorption effect of methylene blue by the ball-milled magnetic biochar prepared in Example 3 of the present invention;
[0038] Fig.12 The absorption effect of different washing methods in repeated absorption of methylene blue by the ball-milled magnetic biochar prepared by the present invention is shown. DETAILED DESCRIPTION
[0039] The following examples are used to demonstrate preferred embodiments of the present invention. It will be appreciated by those skilled in the art that the techniques disclosed in the following examples represent techniques discovered by the inventors that can be used to implement the present invention and therefore can be considered as preferred embodiments of the present invention. However, it will be appreciated by those skilled in the art based on this specification that many modifications may be made to the specific embodiments disclosed herein and still achieve the same or similar results without departing from the spirit or scope of the present invention.
[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs, and the materials cited herein and those cited by them are incorporated by reference. Those skilled in the art will recognize or will learn through routine experimentation that there are many equivalents to the specific embodiments of the invention described herein. Such equivalents are intended to be encompassed by the claims.
[0041] The technical solution of this patent is further described in detail below in conjunction with specific implementation methods.
[0042] Example 1 Screening of biochar
[0043] Wheat straw, rape straw and corn straw were soaked in pure water for 12 h respectively. The washed straw was dried in a 65°C oven. The dried straw was fully ground and sieved through a 60-mesh sieve for later use. The straw powder was pyrolyzed in a 500°C muffle furnace for 3 h with a heating rate of 10°C / min. The biochar after pyrolysis was ground and sieved through a 100-mesh sieve to prepare three types of biochar, which were recorded as BC1, BC2 and BC3 respectively.
[0044] XRD characterization analysis was performed on three types of biochar: wheat straw biochar BC1, rape straw biochar BC2 and corn straw biochar BC3. Figure 1 shown.
[0045] The results showed that the X-ray diffraction spectra of BC1, BC2 and BC3 had obvious diffraction peaks near about 2θ=24°, which were characteristic diffraction peaks belonging to the graphite crystal plane (002), representing the amorphous carbon structure and reflecting the degree of carbonization of biochar.
[0046] 0.02g of BC1, BC2 and BC3 were added to 20mL of 40mg / L methylene blue solution. The pH value of the solution system ranged from 3 to 11, and the adsorption was carried out at 298.15K under constant temperature oscillation for 2h. The results are shown in Figure 2 shown.
[0047] The results showed that as the pH of the methylene blue solution increased, the adsorption of methylene blue by BC1, BC2 and BC3 gradually increased. When pH = 11, the adsorption of methylene blue by BC1, BC2 and BC3 reached the highest, which were 13.14 mg / g, 12.92 mg / g and 12.03 mg / g respectively. It can be seen that the biochar made from wheat straw has the best adsorption effect, so wheat straw biochar was selected for ball milling.
[0048] Example 2 Determination of ball milling parameters for wheat biochar
[0049] The wheat biochar with the best adsorption effect was loaded into an agate ball mill at a mass ratio of 1:20, 1:50, and 1:100, respectively, and then placed on a planetary ball mill for 1 h at 400 r / min and passed through a 100-mesh sieve to obtain three different ball-milled biochars, which were named BM-BC1, BM-BC2, and BM-BC3.
[0050] The adsorption effect of methylene blue on wheat straw ball-milled biochar BM-BC1, BM-BC2, and BM-BC3 was compared: 0.02 g of BM-BC1, BM-BC2, and BM-BC3 were mixed with 50 mL of MB solution with an original pH of 5.65 and a concentration of 100 mg / L, and adsorbed at 298.15 K for 3 h. Figure 3 shown.
[0051] The results showed that the adsorption of methylene blue by BM-BC1, BM-BC2 and BM-BC3 showed a downward trend, and their adsorption amounts were 210.31 mg / g, 118.40 mg / g and 69.61 mg / g, respectively, which were higher than those of pure biochar in Example 1, indicating that ball milling modification improved the adsorption performance of methylene blue to a certain extent. In order to achieve better results in subsequent experiments, BM-BC1 was selected as the research object for the next experiment.
[0052] Example 3 Preparation of BM-Fe3O4 / γ-Fe2O3-BC1
[0053] The preparation of ball-milled magnetic biochar includes the following steps:
[0054] (1) The wheat straw was processed by a crusher, passed through a 100-mesh sieve, and then washed three times with deionized water. Finally, it was placed in a forced air drying oven at 60°C for 12 hours.
[0055] (2) Weigh 4 g of wheat straw powder and 1 g of potassium trioxalatoferrate in a mortar and grind thoroughly.
[0056] (3) The ground mixture is placed in a muffle furnace and calcined to obtain magnetic biochar, wherein the calcination temperature is 500°C and the calcination time is 2 h.
[0057] (4) Finally, the magnetic biochar was ball-milled at 400 r / min for 1 h to obtain the final product, ball-milled magnetic biochar BM-Fe3O4 / γ-Fe2O3-BC1.
[0058] Example 4 Preparation of BM-Fe3O4 / γ-Fe2O3-BC2
[0059] The preparation of ball-milled magnetic biochar includes the following steps:
[0060] (1) The wheat straw was processed by a crusher, passed through a 100-mesh sieve, and then washed three times with deionized water. Finally, it was placed in a forced air drying oven at 60°C for 12 hours.
[0061] (2) Weigh 4 g of wheat straw powder and 2 g of potassium trioxalatoferrate in a mortar and grind thoroughly.
[0062] (3) The ground mixture is placed in a muffle furnace and calcined to obtain magnetic biochar, wherein the calcination temperature is 500°C and the calcination time is 2 h.
[0063] (4) Finally, the magnetic biochar was ball-milled at 400 r / min for 1 h to obtain the final product, ball-milled magnetic biochar BM-Fe3O4 / γ-Fe2O3-BC2.
[0064] Example 5 Preparation of BM-Fe3O4 / γ-Fe2O3-BC3
[0065] The preparation of ball-milled magnetic biochar includes the following steps:
[0066] (1) The wheat straw was processed by a crusher, passed through a 100-mesh sieve, and then washed three times with deionized water. Finally, it was placed in a forced air drying oven at 60°C for 12 hours.
[0067] (2) Weigh 4 g of wheat straw powder and 3 g of potassium trioxalatoferrate in a mortar and grind thoroughly.
[0068] (3) The ground mixture is placed in a muffle furnace and calcined to obtain magnetic biochar, wherein the calcination temperature is 500°C and the calcination time is 2 h.
[0069] (4) Finally, the magnetic biochar was ball-milled at 400 r / min for 1 h to obtain the final product, ball-milled magnetic biochar BM-Fe3O4 / γ-Fe2O3-BC3.
[0070] Performance Comparison
[0071] (1) The biochar BC in Example 1, the biochar BM-BC1 in Example 2, and the biochar BM-Fe3O4 / γ-Fe2O in Example 3 were 3- BC1 was subjected to SEM analysis, and the electron scanning microscope image is shown in Figure 4 shown.
[0072] The results showed that the surface of BC1 showed circular pores with regular shapes and different pore sizes. The existence of the pore structure gave the biochar a certain adsorption capacity. After mechanical ball milling, the surface of BM-BC1 showed irregular and smaller particles, indicating that ball milling modification can effectively reduce the particle size of biochar. 3- BC1 showed an irregular shape and its particle diameter was larger than that of ball-milled biochar BM-BC1, indicating that it was loaded with more iron-containing particles.
[0073] (2) The biochar BC in Example 1, the biochar BM-BC1 in Example 2, and the biochar BM-Fe3O4 / γ-Fe2O in Example 3 3- BC1 was subjected to XRD characterization and the results were compared as shown in Figure 5 shown.
[0074] The results showed that compared with the XRD of BC1, the XRD pattern of BC1 (BM-BC1) after ball milling was highly consistent with the position of the XRD peak of BC1, which indicated that the ball milling treatment did not change the phase composition of BC1. 3- In addition to the characteristic diffraction peaks belonging to the graphite crystal plane (002), the XRD spectrum of BC1 also has characteristic diffraction peaks belonging to Fe3O4 and γ-Fe2O3 at 2θ=30.02°, 35.46°, 43.16°, 53.57°, 56.91° and 62.59°, indicating that the magnetic substance was successfully loaded on the surface of the biochar material.
[0075] (3) The biochar BC in Example 1, the biochar BM-BC1 in Example 2, and the biochar BM-Fe3O4 / γ-Fe2O in Example 3 3-The specific surface area, total pore volume and average pore size of BC1 were compared, and the results are shown in Table 1.
[0076] Table 1BC1, BM-BC1 and BM-Fe3O4 / γ-Fe2O 3- Specific surface area, total pore volume and average pore diameter of BC1
[0077]
[0078] From the above table, we can see that BC1, BM-BC1 and BM-Fe3O4 / γ-Fe2O 3- The specific surface area of BC1 is 12.48m 2 / g, 262.66m 2 / g, 32.91m 2 / g, and the pore volume is 0.015cm 3 / g, 0.227cm 3 / g, 0.033cm 3 / g; the average pore sizes are 4.96nm, 3.43nm, and 3.96nm respectively.
[0079] (4) The ball-milled magnetic biochars prepared in Examples 3 to 5 were subjected to a comparison of methylene blue adsorption, as follows: 0.02 g of BM-Fe3O4 / γ-Fe2O3-BC1, BM-Fe3O4 / γ-Fe2O3-BC2 and BM-Fe3O4 / γ-Fe2O3-BC3 were adsorbed on methylene blue in a solution with an initial methylene blue concentration of 100 mg / L and an original pH of 5.66 for 3 h at a temperature of 298 K. The results are shown in FIG. Figure 6 shown.
[0080] The results showed that the adsorption capacity of methylene blue by BM-Fe3O4 / γ-Fe2O3-BC1, BM-Fe3O4 / γ-Fe2O3-BC2 and BM-Fe3O4 / γ-Fe2O3-BC3 were 245.17, 234.25 and 214.29 mg / g, respectively, which were higher than those of biochar and ball-milled biochar, indicating that ball-milled-magnetic pyrolysis modified biochar can further improve the adsorption performance of methylene blue.
[0081] (5) The ball-milled magnetic biochar prepared in Examples 3 to 5 was subjected to a comparison of methylene blue adsorption under different solution initial concentration conditions, as follows: 0.02 g of BM-Fe3O4 / γ-Fe2O3-BC1 was added to 50 mL of methylene blue solution with initial concentrations of 80 mg / L, 100 mg / L, 120 mg / L, 140 mg / L, 160 mg / L, 180 mg / L, and 200 mg / L, respectively, at pH = 5.66, and the mixture was oscillated at a constant temperature at 298.15 K for 3 h. After filtration, the residual concentration of methylene blue was determined. The results are shown in FIG. Figure 7 shown.
[0082] The results show that as the initial concentration of methylene blue increases, the adsorption of methylene blue by BM-Fe3O4 / γ-Fe2O3-BC1 increases. When the initial concentration of methylene blue is low, there are a large number of adsorption sites on the adsorbent surface that are sufficient to adsorb MB molecules; when the initial concentration of methylene blue is high, the adsorption sites on the adsorbent surface are insufficient to adsorb methylene blue molecules, and the adsorption gradually tends to equilibrium. When the initial concentration of methylene blue is 200 mg / L, the adsorption of MB by BM-Fe3O4 / γ-Fe2O3-BC1 reaches the maximum value, reaching 281.00 mg / g.
[0083] (6) The ball-milled magnetic biochar prepared in Example 3 was compared for the adsorption of methylene blue under different solution pH conditions. The method was as follows: 0.02 g of BM-Fe3O4 / γ-Fe2O3-BC1 was added to 50 mL of a 100 mg / L methylene blue solution, the pH range was set between 3 and 11, and constant temperature oscillation was performed at 298.15 K for 3 h. After the oscillation, the solution was filtered, the residual concentration of methylene blue was determined, and the adsorption amount of methylene blue by BM-Fe3O4 / γ-Fe2O3-BC1 was calculated. The results are shown in Figure 2. Figure 8 shown.
[0084] The results showed that when pH = 3, H+ in the solution formed competitive adsorption with methylene blue molecules. +The adsorption sites on the adsorbent surface were occupied, which reduced the adsorption of methylene blue by BM-Fe3O4 / γ-Fe2O3-BC1. Between pH=5 and 11, as the pH gradually increased, the OH- content in the solution increased, and the surface deprotonation of BM-Fe3O4 / γ-Fe2O3-BC1 promoted the adsorption of methylene blue by BM-Fe3O4 / γ-Fe2O3-BC1. When the pH values were 3, 5, 7, 9, and 11, the adsorption of methylene blue by BM-Fe3O4 / γ-Fe2O3-BC1 was 140.60, 229.34, 242.67, 246.45, and 254.07 mg / g, respectively. As the pH of the solution increased, the adsorption range of methylene blue increased. At the same time, it also showed that the biochar was suitable for different pH environments and had good adsorption performance in acidic, neutral, and even strongly alkaline environments.
[0085] (7) The adsorption of methylene blue by the ball-milled magnetic biochar prepared in Example 3 was investigated over time. The method was as follows: 0.04 g of BM-Fe3O4 / γ-Fe2O3-BC1 was added to 100 mL of a methylene blue solution with a pH of 5.66 and a concentration of 100 mg / L. The solution was oscillated at a constant temperature at 298.15 K for 4 h. The sampling time points were set to 1, 5, 10, 20, 30, 60, 90, 120, 150, 180, and 240 min. 5 mL of the sample solution was filtered each time. The residual concentration of methylene blue was determined and the adsorption amount of methylene blue by BM-Fe3O4 / γ-Fe2O3-BC1 was calculated. The results are shown in Table 1. Fig. 9 shown.
[0086] The results showed that within the first 30 minutes, the adsorption of methylene blue by BM-Fe3O4 / γ-Fe2O3-BC1 increased with time; after 30 minutes, the adsorption effect of BM-Fe3O4 / γ-Fe2O3-BC1 on methylene blue gradually increased and eventually tended to equilibrium. The content of active sites on the adsorbent surface determined the adsorption rate. The adsorption reached equilibrium at 150 minutes. At 240 minutes, the adsorption effect of BM-Fe3O4 / γ-Fe2O3-BC1 on methylene blue reached the best, with an adsorption amount of 238.05 mg / g.
[0087] (8)BM-Fe3O4 / γ-Fe2O 3- Magnetic analysis of BC1: The magnetic properties of BM-Fe3O4 / γ-Fe2O3-BC1 were measured by VSM analysis at room temperature. The hysteresis loop of BM-Fe3O4 / γ-Fe2O3-BC1 is shown above. Fig.10 shown.
[0088] The results show that the saturation magnetization intensity of biochar BM-Fe3O4 / γ-Fe2O3-BC1 is 15.30emu / g, which has strong paramagnetism. Fig.10 The internal inset shows that BM-Fe3O4 / γ-Fe2O3-BC1 is easily attracted by the external magnetic field alone, indicating that the separation of BM-Fe3O4 / γ-Fe2O3-BC1 from methylene blue solution can be achieved under the condition of an external magnetic field.
[0089] (9) BM-Fe3O4 / γ-Fe2O prepared in Example 3 3- The repeated absorption effect of BC1 on methylene blue was as follows: 0.02 g of BM-Fe3O4 / γ-Fe2O 3- BC1, the initial concentration of methylene blue is 100 mg / L, pH=5.66, the volume is 50 mL, and 3 parallel samples are set. Constant temperature oscillation is carried out at 298.15K for 3 hours. After the adsorption is completed, the residual concentration of methylene blue is measured, and the calculated adsorption amount is the adsorption amount of the first cycle. The adsorbed material is recycled by magnet, and the adsorbed material is washed several times with anhydrous ethanol and 0.01 mol / L dilute hydrochloric acid solution, and then used for the second adsorption, and so on. The recycling effect is as follows Fig.11 shown.
[0090] The results show that: BM-Fe3O4 / γ-Fe2O 3- After BC1 was recycled three times, its adsorption capacity could reach 196.57 mg / g; compared with the initial adsorption capacity, its adsorption capacity only decreased by 14.39%.
[0091] In addition, during the research process, we found that the cleaning method of the adsorbed material before reuse affects the repeated absorption effect of the material: after cleaning with anhydrous ethanol, BM-Fe3O4 / γ-Fe2O 3- BC1 was recycled 3 times, and its adsorption capacity was 230.79 mg / g. Fig.12 shown.
[0092] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as references separately. In addition, it should be understood that after reading the above teachings of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined in the present application.
Claims
1. A method for mechanochemical modification of magnetic biochar by ball milling, characterized in that: The steps include: (1) The biomass raw material is processed by a crusher, sieved, then fully washed with deionized water, and placed in a drying oven to completely dry; (2) placing the biomass raw material powder and potassium trioxalatoferrate in a mortar at a mass ratio of 4:(1-3) and grinding them thoroughly; (3) placing the ground mixture in a muffle furnace and calcining it to obtain magnetic biochar; (4) The magnetic biochar is ball-milled to obtain the final product, ball-milled magnetic biochar.
2. The method for mechanochemical modification of magnetic biochar by ball milling according to claim 1, characterized in that: The biomass raw material is wheat straw.
3. The method for mechanochemical modification of magnetic biochar by ball milling according to claim 1, characterized in that: The calcination temperature is 500-600° C. and the calcination time is 2-3 hours.
4. The method for mechanochemical modification of magnetic biochar by ball milling according to claim 1, characterized in that: The ball milling conditions are: rotation speed 400-500 r / min, processing time 1-2 h.
5. The method for mechanochemical modification of magnetic biochar by ball milling according to claim 1, characterized in that: The mass ratio of the magnetic biochar to the ball milling beads in the ball mill is 1:(15-25).
6. The method for mechanochemical modification of magnetic biochar by ball milling according to claim 1, characterized in that: The drying oven is a blast drying oven, the blast drying oven temperature is 50-60° C., and the drying time is 8-12 hours.
7. A magnetic biochar, characterized in that: The magnetic biochar is prepared by the method according to any one of claims 1 to 6.
8. Use of the magnetic biochar prepared by the method according to any one of claims 1 to 6 in adsorbing organic dye wastewater.
9. The use according to claim 8, characterized in that: The magnetic biochar is placed in wastewater containing organic dyes, and the pH value of the organic dye wastewater is 3-12.
10. The use according to claim 8, characterized in that: The adsorbed magnetic biochar is recovered by magnetic absorption and then washed multiple times with anhydrous ethanol and 0.01 mol / L dilute hydrochloric acid solution before reuse.