Water self-cleaning catalyst for activating dissolved oxygen and preparation method thereof
By using the catalyst CCQds-CN that activates dissolved oxygen in water treatment, the problem of traditional water treatment technology poor removal of new pollutants is solved, efficient degradation under normal temperature and pressure is achieved, energy consumption is reduced, and it is shown that Prove good cycle stability and application prospects.
Patent Information
- Application Number
- CN202411151704.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional water treatment technology is not effective in removing new pollutants such as endocrine interferons, antibiotics, persistent organic pollutants and microplastics in the water. Advanced oxidation technology consumes a lot of chemicals and energy, resulting in high energy consumption in the water treatment process.
Develop a self-purification catalyst for activation of dissolved oxygen. The catalyst CCQds-CN can be prepared by polymerizing 2-methylimidazole with zinc salt, cobalt salt and copper salt in an alcohol solvent, and calcination and annealing treatment, which can be prepared at room temperature. Effectively degrade new pollutants under normal pressure, without the need for additional energy and agents.
The catalyst steadily degrades new pollutants under wide pH range and different salt conditions, significantly reducing resource and energy consumption in the water treatment process, and has a significant effect on removing new pollutants such as BPA, PHT, IBU, etc. in wastewater, with a long service life , has good prospects for cycle application.
Smart Images

Figure CN119034779A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of sewage treatment, and in particular to a water self-purification catalyst for activating dissolved oxygen and a preparation method thereof. Background Art
[0002] With the growth of the global population and economic development, the demand for water resources continues to increase, but the supply of water resources is limited by various factors, resulting in clean and safe water being a challenge. According to tests, new pollutants such as endocrine disruptors, antibiotics, persistent organic pollutants and microplastics are widely present in natural water bodies. Due to the enrichment of the food chain, even trace amounts of new pollutants in water bodies can pose a threat to aquatic life and public health. Therefore, removing these new pollutants from water is very important and urgent to avoid long-term exposure to humans and organisms. Traditional water treatment technology has little effect on the removal of new pollutants. Although advanced oxidation technology can effectively remove new pollutants that are difficult to degrade in water, it requires a large amount of chemical agents and energy.
[0003] Therefore, there is an urgent need to develop a new water treatment material to achieve zero external consumption self-purification of new pollutants in water bodies at normal temperature and pressure, thereby reducing energy consumption in the sewage treatment process. Summary of the invention
[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a water self-purification catalyst for activating dissolved oxygen and a preparation method thereof. The catalyst has a stable effect, does not require additional energy and reagents, can effectively degrade new pollutants under room temperature conditions in a wide pH range and in the presence of different salts, greatly reduces resource and energy consumption in the water treatment process, and has good application prospects.
[0005] The purpose of the present invention is achieved by adopting the following technical solutions:
[0006] In a first aspect, the present invention provides a method for preparing a water self-purification catalyst for activating dissolved oxygen, comprising the following steps:
[0007] S1, dissolving 2-methylimidazole and zinc salt in an alcohol organic solvent, then adding cobalt salt and copper salt to carry out polymerization reaction, filtering out the solid product after the reaction, washing and drying to obtain a precursor;
[0008] S2. Grind the precursor and perform calcination and annealing treatment, grind it again, wash and dry it to obtain the catalyst CCQds-CN.
[0009] Preferably, in S1, the zinc salt is zinc sulfate, the cobalt salt is cobalt nitrate, and the copper salt is copper nitrate.
[0010] Preferably, in S1, the molar ratio of 2-methylimidazole, zinc salt, cobalt salt and copper salt is 0.01-0.1: 0.01-0.06: 0.001-0.005: 0.001-0.005.
[0011] Preferably, in S1, the molar ratio of 2-methylimidazole, zinc salt, cobalt salt and copper salt is 0.04-0.08: 0.02-0.05: 0.002-0.005: 0.002-0.005.
[0012] Preferably, in S1, the molar ratio of 2-methylimidazole, zinc salt, cobalt salt and copper salt is 0.05-0.07: 0.03-0.05: 0.002-0.004: 0.003-0.004.
[0013] Preferably, in S1, the molar ratio of 2-methylimidazole, zinc salt, cobalt salt and copper salt is 0.07:0.04:0.003:0.004.
[0014] Preferably, in S1, the alcohol organic solvent is selected from at least one of methanol, ethanol and isopropanol.
[0015] Preferably, in S1, the polymerization reaction temperature is 20-40° C., and the polymerization reaction time is 20-30 h.
[0016] Preferably, in S1, the filtration is centrifugal filtration, the rotation speed during centrifugal filtration is 7000-10000rpm, and the centrifugal filtration time is 5-10min; the washing is carried out alternately with deionized water and anhydrous ethanol, and the number of washing times is 3-10 times; the drying is carried out in a vacuum drying oven; the drying temperature is 60-80°C, and the drying time is 8-12h.
[0017] Preferably, in S2, the calcination and annealing is carried out in a tubular furnace in a nitrogen atmosphere, the calcination and annealing temperature is 500-900°C, the calcination time is 1-3h, and the heating rate during calcination is 5-10°C / min.
[0018] Preferably, in S2, the calcination annealing temperature is 700-900°C, more preferably 800°C.
[0019] Preferably, in S2, the particle size of the precursor ground is 50-100 mesh; washing is performed alternately with deionized water and anhydrous ethanol, and the number of washing times is 3-10 times; the drying temperature is 60-80° C., and the drying time is 3-5 hours.
[0020] In a second aspect, the present invention provides a water self-purification catalyst for activating dissolved oxygen, which is prepared according to the above preparation method.
[0021] In a third aspect, the present invention provides a water self-purification catalyst for activating dissolved oxygen and its use in treating new pollutants in water.
[0022] Preferably, the new pollutants in the water include bisphenol A (BPA), phenytoin (PHT), ibuprofen (IBU), sulfamethoxazole (SMZ), and ciprofloxacin (CIP); the concentration of the new pollutants in the water is ≥1ppm; and the amount of the catalyst used when treating the new pollutants in the water is 0.6-1.4g / L.
[0023] The beneficial effects of the present invention are:
[0024] 1. The catalyst preparation method of the present invention is simple, has low equipment requirements, and has a short implementation period. When treating new pollutants in sewage, it can adapt to a wider pH range and still have a good removal effect on new pollutants in the presence of different salts.
[0025] 2. The catalyst of the present invention can activate dissolved oxygen in water at normal temperature and pressure, forming a self-purification system in sewage. In the process of removing new pollutants in water, no additional energy and agents are required, which greatly reduces the resource and energy consumption in the water treatment process;
[0026] 3. The catalyst of the present invention is a solid catalyst with a special structure and excellent pollutant adsorption and degradation effects. In the application case, it has a significant effect on removing new pollutants such as BPA, PHT, CIP, IBU, etc. in wastewater.
[0027] 4. The catalyst of the present invention has good stability, long service life, is easy to recycle and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The present invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.
[0029] Figure 1 This is a transmission electron microscopy (TEM) image of the water self-purification catalyst for activating dissolved oxygen prepared in Example 1.
[0030] Figure 2 These are the degradation curves of BPA, PHT, IBU, SMZ, and CIP of the water self-purification catalyst for activating dissolved oxygen prepared in Example 1.
[0031] Figure 3 This is the degradation curve of CIP of the water self-purification catalyst for activating dissolved oxygen prepared in Example 1 in the presence of different anions.
[0032] Figure 4This is a diagram showing the cyclic stability of the water self-purification catalyst used to activate dissolved oxygen prepared in Example 1. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0034] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0035] The present invention will be further described below in conjunction with the following examples.
[0036] Example 1
[0037] A method for preparing a water self-purification catalyst for activating dissolved oxygen comprises the following steps:
[0038] S1: 2-methylimidazole and zinc sulfate were dissolved in 120 ml of methanol, and then cobalt nitrate and copper nitrate were added for polymerization reaction for 24 hours. After the reaction, the solid product was filtered out, washed alternately with deionized water and anhydrous ethanol for 6 times, and then vacuum dried at 60°C for 12 hours to obtain a precursor. The molar ratio of 2-methylimidazole, zinc nitrate, cobalt nitrate and copper nitrate was controlled to be 0.07:0.04:0.003:0.004.
[0039] S2: The precursor was ground to 80 mesh, and then a tube furnace was used to complete the calcination-annealing process in a N2 atmosphere, specifically, the temperature was raised to 900℃ at a rate of 5℃ / min for 1h, and the product was taken out after natural cooling. After grinding again, washing, and drying, the catalyst CCQds-CN was obtained, and its transmission electron microscopy (TEM) image is shown as follows: Figure 1 shown.
[0040] Example 2
[0041] A method for preparing a water self-purification catalyst for activating dissolved oxygen comprises the following steps:
[0042] S1: 2-methylimidazole and zinc sulfate were dissolved in 120 ml of methanol, and then cobalt nitrate and copper nitrate were added for polymerization reaction for 24 hours. After the reaction, the solid product was filtered out, washed alternately with deionized water and anhydrous ethanol for 6 times, and then vacuum dried at 60°C for 12 hours to obtain a precursor. The molar ratio of 2-methylimidazole, zinc nitrate, cobalt nitrate and copper nitrate was controlled to be 0.06:0.04:0.003:0.004.
[0043] S2: The precursor was ground to 80 mesh, and then a tubular furnace was used to complete the calcination-annealing procedure in a N2 atmosphere, specifically, the temperature was raised to 900°C at a rate of 5°C / min for 1 hour, and the product was taken out after natural cooling. After grinding again, washing, and drying, the catalyst CCQds-CN-1 was obtained.
[0044] Example 3
[0045] A method for preparing a water self-purification catalyst for activating dissolved oxygen comprises the following steps:
[0046] S1: 2-methylimidazole and zinc sulfate were dissolved in 120 ml of methanol, and then cobalt nitrate and copper nitrate were added for polymerization reaction for 24 hours. After the reaction, the solid product was filtered out, washed alternately with deionized water and anhydrous ethanol for 6 times, and then vacuum dried at 60°C for 12 hours to obtain a precursor. The molar ratio of 2-methylimidazole, zinc nitrate, cobalt nitrate and copper nitrate was controlled to be 0.06:0.05:0.003:0.004.
[0047] S2: The precursor was ground to 80 mesh, and then a tubular furnace was used to complete the calcination-annealing procedure in a N2 atmosphere, specifically, the temperature was raised to 900°C at a rate of 5°C / min for 1 hour, and the product was taken out after natural cooling. After grinding again, washing, and drying, the catalyst CCQds-CN-2 was obtained.
[0048] Application Example 1
[0049] The water self-purification catalyst for activating dissolved oxygen prepared in Example 1 was used to degrade new pollutants in water, and its degradation effect on different pollutants was tested; the details are as follows:
[0050] 0.03 g of the catalyst (CCQds-CN) of Example 1 was added to 50 mL of 1 ppm solution of different types of pollutants, kept at a constant temperature of 35° C., stirred continuously, and samples were taken at different time points to detect changes in the concentration of pollutants; the results are as follows: Figure 2 As shown:
[0051] Figure 2The results showed that the degradation effect of SMZ reached 100% within 30 minutes, and the degradation effects of BPA, PHT, IBU and CIP reached about 77%, 96%, 100% and 99% respectively within 120 minutes. The degradation effect of the catalyst on the pollutants SMZ and CIP was more prominent.
[0052] Application Example 2
[0053] The water self-purification catalyst for activating dissolved oxygen prepared in Example 1 was used to remove new pollutants CIP in water under the interference of anions; the details are as follows:
[0054] 0.03 g of the catalyst (CCQds-CN) of Example 1 was added to the following mixtures: - 、HCO3 - 、HPO4 2- 、NO3 - 、SO4 2- The new pollutant CIP solution of 50mL and 1ppm was kept at a constant temperature of 35℃ and stirred continuously. Samples were taken at different time points to detect the concentration changes of pollutants. The results are as follows Figure 3 shown.
[0055] Figure 3 The results show that in the presence of different anions, the removal effect of the catalyst (CCQds-CN) on CIP remains stable, that is, the presence of anions in the solution has no obvious effect on the degradation of CIP.
[0056] Application Example 3
[0057] The water self-purification catalyst for activating dissolved oxygen prepared in Example 1 was used to degrade the new pollutant CIP in water, and its cyclic stability in removing CIP in aqueous solution was tested; the details are as follows:
[0058] (1) Take 0.03g of the catalyst (CCQds-CN) of Example 1 and add it to 50mL of 1ppm new pollutant CIP solution, keep the temperature at 35℃, stir continuously, and take samples at different time points to detect the concentration change of the pollutant; (2) Filter the solution after the reaction, take the catalyst obtained by filtration, dry it and recycle it, and evaluate the activity of step (1); (3) Repeat step (2). Repeat the detection of the initial concentration of ciprofloxacin during the reaction and the concentration after the reaction to determine the stability and repeatability of the catalyst; the results are as follows: Figure 4 As shown:
[0059] Figure 4The results show that the catalyst continued to react for multiple cycles without a significant decrease in its degradation activity for CIP. After six cycles of reaction, its removal rate for CIP within a given time remained at 85%, indicating that the catalyst has good stability and repeatability.
[0060] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0061] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a water self-purification catalyst for activating dissolved oxygen, characterized in that: The following steps are involved: S1, dissolving 2-methylimidazole and zinc salt in an alcohol organic solvent, then adding cobalt salt and copper salt to carry out polymerization reaction, filtering out the solid product after the reaction, washing and drying to obtain a precursor; S2. Grind the precursor and perform calcination and annealing treatment, grind it again, wash and dry it to obtain the catalyst CCQds-CN.
2. The method for preparing a water self-purification catalyst for activating dissolved oxygen according to claim 1, characterized in that: In S1, the zinc salt is zinc sulfate, the cobalt salt is cobalt nitrate, and the copper salt is copper nitrate; the molar ratio of 2-methylimidazole, zinc salt, cobalt salt and copper salt is 0.01-0.1: 0.01-0.06: 0.001-0.005: 0.001-0.
005.
3. The method for preparing a water self-purification catalyst for activating dissolved oxygen according to claim 1, characterized in that: In S1, the alcohol organic solvent is selected from at least one of methanol, ethanol and isopropanol.
4. The method for preparing a water self-purification catalyst for activating dissolved oxygen according to claim 1, characterized in that: In the step S1, the polymerization reaction temperature is 20-40° C., and the polymerization reaction time is 20-30 h.
5. The method for preparing a water self-purification catalyst for activating dissolved oxygen according to claim 1, characterized in that: In S1, the filtration is centrifugal filtration, the rotation speed during the centrifugal filtration is 7000-10000rpm, and the centrifugal filtration time is 5-10min; the washing is carried out alternately with deionized water and anhydrous ethanol, and the number of washing times is 3-10 times; the drying is carried out in a vacuum drying oven; the drying temperature is 60-80°C, and the drying time is 8-12h.
6. The method for preparing a water self-purification catalyst for activating dissolved oxygen according to claim 1, characterized in that: In S2, the calcination and annealing are carried out in a tubular furnace in a nitrogen atmosphere, the calcination and annealing temperature is 500-900°C, the calcination time is 1-3h, and the heating rate during calcination is 5-10°C / min.
7. The method for preparing a water self-purification catalyst for activating dissolved oxygen according to claim 1, characterized in that: In S2, washing is performed alternately with deionized water and anhydrous ethanol, and the number of washing times is 3-10 times; the drying temperature is 60-80° C., and the drying time is 3-5 hours.
8. A water self-purification catalyst for activating dissolved oxygen, characterized in that: The preparation method according to claim 1 is used for preparation.
9. Use of the water self-purification catalyst for activating dissolved oxygen according to claim 8 in treating new pollutants in water.
10. Use of a water self-purification catalyst for activating dissolved oxygen in treating new pollutants in water according to claim 9, characterized in that: The new pollutants in the water include bisphenol A, phenytoin, ibuprofen, sulfamethazole, and ciprofloxacin; the concentration of the new pollutants in the water is ≥1ppm; and the dosage of the catalyst when treating the new pollutants in the water is 0.6-1.4g / L.