Transition metal-noble metal dual-alloy catalyst and preparation method thereof

By preparing transition metal-precious metal dual alloy catalysts, using their multiple oxidation states and chemically active sites, combined with the domain-limiting effect of molecular sieve, the problem of active sites agglomeration of precious metal catalysts under high temperature conditions is solved, and efficient and economical Tritium removal is suitable for deep oxidation removal of low-concentration hydrogen isotope gases under low temperature conditions.

CN119034799APending Publication Date: 2024-11-29SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411161239.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The active sites of existing precious metal catalysts are prone to agglomeration under high temperature conditions, resulting in a decrease in catalytic performance. The high cost of precious metals limits their large-scale industrial applications, making it difficult to effectively remove tritium from tritium-containing waste gas.

Method used

Using transition metal-precious metal dual alloy catalysts, it is synthesized by hydrothermal method and uses molecular sieve as a support. It uses a variety of oxidation states and chemically active sites of transition metals and noble metals, and combines the domain-limiting effect of molecular sieve to prepare efficient catalysts to prevent Reunites reunite and reduce costs.

Benefits of technology

It realizes flexibility and efficient catalytic performance under different reaction conditions, reduces the cost of industrial applications, improves the efficiency of tritium removal, and is suitable for the deep oxidation removal of low-concentration hydrogen isotope gases under low temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034799A_ABST
    Figure CN119034799A_ABST
Patent Text Reader

Abstract

The invention discloses a transition metal-precious metal dual-alloy catalyst and a preparation method thereof.The method comprises the steps that a, a transition metal source, a precious metal source and a molecular sieve precursor solution are mixed, and a preliminary catalyst is synthesized through a hydrothermal method; wherein transition metal contained in the transition metal source is one or more of Fe, Co, Ni, Cu, Zn, Sn and Mn oxides, and precious metal contained in the precious metal source is one or more of Pt, Pd, Ru and Rh; and b, sequentially cleaning, drying, calcining and reducing the primary catalyst to obtain the transition metal-noble metal dual-alloy catalyst. The transition metal-noble metal dual-alloy catalyst obtained by the method is a catalyst which takes a molecular sieve as a carrier and takes transition metal and noble metal as active sites. The catalyst prepared by the invention realizes efficient catalytic oxidation removal of hydrogen isotopes, is beneficial to environmental protection and human health, and also can promote sustainable development of tritium-related engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of waste gas treatment, and in particular to a transition metal-noble metal dual alloy catalyst and a preparation method thereof. Background Art

[0002] Tritium, as an isotope gas of hydrogen, has a certain degree of radioactivity (β decay, half-life is 12.43 years). During the operation, maintenance and decommissioning of tritium-containing equipment, leakage of tritium-containing radioactive gas is inevitable. Therefore, the effective removal of tritium from tritium-containing waste gas is crucial to the safety of the public and the environment, and is of great significance to the sustainable development of human society. Catalytic oxidation has become an important method for detritiation due to its high efficiency and deep oxidation of tritium. The oxidized tritium water is easier to recover and treat. The improvement of catalytic oxidation efficiency depends on the development of efficient catalysts. Precious metals show high catalytic activity, especially the ability to efficiently decompose hydrogen isotope gases. For example, Pt-based catalysts (such as Pt@CDM and HisoNCat) have been used for the catalytic oxidation treatment of hydrogen isotope gases H2 and D2 (simulating T2).

[0003] Although precious metals exhibit good catalytic oxidation performance, due to their high cost and limited resources, higher amounts of precious metals increase costs and hinder large-scale industrial applications. At the same time, the active sites of precious metals in some existing catalysts tend to agglomerate under high temperature conditions, resulting in a reduction in the number of active sites and a decrease in performance. Summary of the invention

[0004] In view of the above problems, the present invention proposes a transition metal-noble metal dual alloy catalyst and a preparation method thereof.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A method for preparing a transition metal-noble metal dual alloy catalyst comprises the following steps:

[0007] Step a, mixing a transition metal source, a noble metal source and a molecular sieve precursor solution, and synthesizing a preliminary catalyst by a hydrothermal method; wherein the transition metal contained in the transition metal source is one or more of Fe, Co, Ni, Cu, Zn, Sn, and Mn oxides, and the noble metal contained in the noble metal source is one or more of Pt, Pd, Ru, and Rh metals;

[0008] Step b, washing, drying, calcining and reducing the preliminary catalyst in sequence to obtain a powdery transition metal-noble metal dual alloy catalyst.

[0009] Furthermore, the transition metal source is a ligand-protected transition metal salt solution, and the noble metal source is an organic ligand-protected noble metal salt solution, wherein the ligand-protected solution is any one of ethylenediamine, dimethyldiethylamine, diethylenetriamine, and acetylacetone; the molar ratio between the transition metal salt and the organic ligand in the transition metal salt is 1:(15-35); the molar ratio between the noble metal salt and the organic ligand in the noble metal salt solution is 1:(10-30).

[0010] Furthermore, the molecular sieve precursor solution consists of a silicon source, a template and deionized water.

[0011] Furthermore, the silicon source is any one or more of tetraethoxysilane, methyltriethoxysilane, methyltripropoxysilane and trimethoxysilane; the template is any one of tetrapropylammonium hydroxide, tetrapropylammonium bromide and n-butylamine; and the molar ratio of the silicon source, the template and deionized water is 1:(0.3-0.7):(33-66).

[0012] Furthermore, the temperature of the hydrothermal synthesis is 120-170°C; and the synthesis time is 24-96h.

[0013] Furthermore, the cleaning method in step b is centrifugation, and the centrifugal speed is 5000-8000rpm; the cleaning solvent is ethanol or deionized water, the cleaning time is 30-60min, and the final washing is until the pH is neutral; the drying temperature is 50-100℃; the calcination temperature is 450-600℃; the reduction temperature is 350-550℃, and the reducing gas is at least one of H2 and Ar.

[0014] Further, the cleaning is performed by a centrifugal cleaning device, the centrifugal cleaning device comprising:

[0015] The cylinder body has a cleaning chamber with an upper opening and a mounting chamber located below the cleaning chamber, wherein the cleaning chamber and the mounting chamber are separated by a bottom plate, and a drainage port is provided on a side wall of the bottom plate or the mounting chamber;

[0016] A driving member is rotatably mounted on the cylinder, the upper end of the driving member is located at the bottom of the cleaning chamber, and the lower end of the driving member is located in the mounting chamber;

[0017] A driving motor, located in the mounting cavity, for driving the driving member to rotate;

[0018] A container for accommodating objects to be cleaned, the container comprising a cylindrical screen and reinforcing sleeves respectively fixed to the upper and lower ends of the cylindrical screen, the side wall and the bottom wall of the cylindrical screen being both mesh structures, the reinforcing sleeve at the lower end of the container being used to seal the outer sleeve on the upper end of the driving member, a rotating clamping structure being provided between the reinforcing sleeve and the driving member, and the container being able to rotate synchronously when the motor drives the driving member to rotate;

[0019] a first water pipe, sealingly passing through the driving member and used for injecting water into the space formed by the driving member and the receiving member, wherein the driving member is rotatable relative to the first water pipe;

[0020] a water pump, installed on the first water pipe;

[0021] A second water pipe, one end of which is connected to the drain port and is used to drain the water in the installation cavity;

[0022] A sealing cover, detachably mounted on the upper end of the cylinder, for covering the opening of the cleaning chamber;

[0023] A rotating plug is rotatably mounted on the side of the cover facing the cleaning chamber through a bearing, and the rotating plug is used for sealing a reinforcing sleeve disposed on the upper end of the receiving member. When working, the rotating axes of the rotating plug, the receiving member and the driving member coincide with each other;

[0024] The pH detection sensor is arranged in the installation cavity and is used to detect the pH value of the liquid in the cylinder.

[0025] Furthermore, the preparation method further comprises step c, molding the powdered transition metal-noble metal dual alloy catalyst, the specific method being:

[0026] The powdered transition metal-noble metal dual alloy catalyst obtained in step b is uniformly dispersed in a mixed solution of sodium alginate and deionized water, the mixed solution is poured into a mold, cooled with liquid nitrogen and allowed to stand in the air for a certain period of time, and the mold is removed; the obtained granular catalyst is freeze-dried to obtain a regularized transition metal-noble metal dual alloy catalyst that follows the shape of the mold.

[0027] Furthermore, the molar ratio of sodium alginate to deionized water is 1:(300-400); the glass template mold has an outer diameter of 5-30 mm and an inner diameter of 3-28 mm, the freeze-drying temperature is -40--10°C, and the freeze-drying time is 12-24 hours.

[0028] The technical solution of the present invention also discloses a transition metal-noble metal dual alloy catalyst, which is a catalyst prepared by using a molecular sieve as a carrier and a transition metal and a noble metal as active sites; wherein the transition metal is one or more of Fe, Co, Ni, Cu, Zn, Sn, and Mn oxides, and the noble metal is one or more of Pt, Pd, Ru, and Rh metals.

[0029] Furthermore, the transition metal-noble metal dual alloy catalyst is based on weight, the transition metal loading is 0.1-2wt.%, the noble metal loading is 0.1-2wt.%, and the prepared molecular sieve is a hydrophobic pure silicon molecular sieve, and the types of the pure silicon molecular sieve include MFI, FAU, and CHA.

[0030] The beneficial effects of the present invention are as follows: transition metal oxides can exist in a variety of oxidation states, which makes them have good flexibility and adaptability under different reaction conditions. Its diverse oxidation states can promote redox reactions, so that it exhibits excellent performance in the catalytic process. At the same time, the surface of transition metal oxides has abundant chemical active sites, which can adsorb and activate various reactant molecules and improve the efficiency of catalytic reactions. More importantly, compared with precious metal catalysts, transition metal oxides are generally more economical and reduce the cost burden in industrial applications. Combined with the confinement effect of molecular sieves, the agglomeration of active sites under high temperature conditions can be effectively prevented. Considering the importance of tritium safety engineering, the development of catalysts with efficient tritium removal performance is still a direction to be explored.

[0031] Therefore, the present invention develops a transition metal-noble metal dual alloy molecular sieve catalyst and optimizes its preparation method to achieve efficient catalytic oxidation removal of hydrogen isotopes, which not only contributes to environmental protection and human health, but also promotes the sustainable development of tritium-related projects. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The XRD results of the molecular sieve confined transition metal Co and noble metal Pt catalyst in Example 1;

[0033] Figure 2 FT-IR results of the molecular sieve confined transition metal Ni and noble metal Pt catalyst in Example 2;

[0034] Figure 3a TEM results of the molecular sieve confined transition metal Cu and noble metal Pt catalyst in Example 3;

[0035] Figure 3b The particle size distribution results of the molecular sieve confined transition metal Cu and noble metal Pt catalysts in Example 3;

[0036] Figure 4a TEM results of the molecular sieve-confined transition metal Zn and noble metal Pt catalyst in Example 4;

[0037] Figure 4b The particle size distribution results of the molecular sieve confined transition metal Zn and precious metal Pt catalyst in Example 4;

[0038] Figure 5aTEM results of the molecular sieve-confined transition metal Mn and noble metal Pt catalyst in Example 5;

[0039] Figure 5b The particle size distribution results of the molecular sieve confined transition metal Mn and precious metal Pt catalyst in Example 5;

[0040] Figure 6 The restart performance test results of the molecular sieve confined transition metal Cu and noble metal Pt catalysts in Example 6;

[0041] Figure 7 is a schematic diagram of the centrifugal cleaning device when the cover is installed on the cylinder;

[0042] Figure 8 is a schematic diagram of the centrifugal cleaning device after the capping device is removed from the cylinder;

[0043] Fig. 9 is a top view of the centrifugal cleaning device after the cover is hidden;

[0044] Fig.10 yes Fig. 9 AA section view;

[0045] Fig.11 It is a schematic diagram of the cylinder after the cover is hidden;

[0046] Fig.12 yes Fig.11 Schematic diagram after the receiving part and the driving part are separated.

[0047] The reference numerals in the figures are:

[0048] 1. Cylinder; 11. Cleaning chamber; 12. Bottom plate; 13. Installation chamber; 14. Drain port; 15. Positioning hole; 2. Driving member; 21. First conical portion; 22. Positioning portion; 221. Anti-slip groove; 3. Driving motor; 4. Receiving member; 41. Cylindrical screen; 42. Reinforcement sleeve; 421. Connecting portion; 422. Protrusion; 51. First water pipe; 52. Water pump; 53. Second water pipe; 6. Sealing cap; 61. Rotating plug; 611. Second conical portion; 62. Positioning column; 7. pH detection sensor. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments.

[0050] Example 1

[0051] Embodiment 1 of the present invention comprises the following steps:

[0052] Step a1, 0.5 mL of 0.09 M ethylenediamine coordinated Co transition metal solution, 0.5 mL of 0.09 M ethylenediamine coordinated Pt noble metal solution and 7.5 g of deionized water were uniformly mixed by magnetic stirring for 30 min. Then 6.5 g of template agent tetrapropylammonium hydroxide and 4.2 g of silicon source tetraethoxysilane solution were added to the mixed solution, and magnetic stirring was performed for 6 h.

[0053] Step b2, transfer the preliminary solution obtained by mixing after magnetic stirring to a reactor, hydrothermally heat at 170°C, and react for 72 hours. Use deionized water for repeated centrifugation, the centrifugal speed is 8000rpm, the centrifugal washing time is 60 minutes, and finally wash until the pH is neutral. Dry the centrifuged catalyst at 80°C for 12 hours. Calcine the obtained powder material at 550°C in an air atmosphere for 6 hours, and then reduce it at 400°C in a H2 / Ar atmosphere for 2 hours. Obtain a transition metal-noble metal dual alloy catalyst, such as Figure 1 As shown by XRD, the catalyst is mainly MFI type pure silicon molecular sieve.

[0054] One application of this embodiment is: 50 mg of the catalyst obtained in this embodiment is used to catalytically oxidize and remove hydrogen from a mixed gas of oxygen, nitrogen and hydrogen. The hydrogen concentration is 2000 ppm, the reaction temperature is 50°C, and the reaction time space velocity is 48000 mL·g -1 ·h -1 The space velocity was 1.5 ℃ and the stable hydrogen oxidation removal rate was 99.9%.

[0055] Example 2

[0056] Embodiment 2 of the present invention comprises the following steps:

[0057] Step a2, 0.5 mL of 0.09 M ethylenediamine coordinated Ni transition metal solution, 0.5 mL of 0.09 M ethylenediamine coordinated Pt noble metal solution and 7.5 g of deionized water were uniformly mixed by magnetic stirring for 30 min. Then 6.5 g of template agent tetrapropylammonium hydroxide and 4.2 g of silicon source tetraethoxysilane solution were added to the mixed solution, and magnetic stirring was performed for 6 h.

[0058] Step b2, transfer the solution obtained by magnetic stirring to a reactor, hydrothermally heat at 170°C, and react for 72 hours. Use deionized water for repeated centrifugation, the centrifugal speed is 8000rpm, the centrifugal washing time is 60 minutes, and finally wash until the pH is neutral. Dry the centrifuged catalyst at 80°C for 12 hours. Calcine the obtained powder material at 550°C in an air atmosphere for 6 hours, and then reduce it at 400°C in a H2 / Ar atmosphere for 2 hours. Obtain a transition metal-noble metal dual alloy catalyst, such as Figure 2The infrared results show that the catalyst is mainly MFI type pure silicon molecular sieve.

[0059] One application of this embodiment is: 50 mg of the catalyst obtained in this embodiment is used to catalytically oxidize and remove hydrogen from a mixed gas of oxygen, nitrogen and hydrogen. The hydrogen concentration is 2000 ppm, the reaction temperature is 50°C, and the reaction time space velocity is 48000 mL·g -1 ·h -1 The space velocity was 1.53°, and a stable hydrogen oxidation removal efficiency of 96.1% was obtained.

[0060] Example 3

[0061] Embodiment 3 of the present invention comprises the following steps:

[0062] Step a3, 0.5 mL of 0.09 M ethylenediamine-coordinated Cu transition metal solution, 0.5 mL of 0.09 M ethylenediamine-coordinated Pt noble metal solution and 7.5 g of deionized water were uniformly mixed by magnetic stirring for 30 min. Then 6.5 g of template agent tetrapropylammonium hydroxide and 4.2 g of silicon source tetraethoxysilane solution were added to the mixed solution, and magnetic stirring was performed for 6 h.

[0063] Step b3, transfer the solution obtained by magnetic stirring to a reactor, hydrothermally heat at 170°C, and react for 72 hours. Use deionized water for repeated centrifugation, the centrifugal speed is 8000rpm, the centrifugal washing time is 60 minutes, and finally wash until the pH is neutral. Dry the centrifuged catalyst at 80°C for 12 hours. Calcine the obtained powder material at 550°C in an air atmosphere for 6 hours, and then reduce it at 400°C in a H2 / Ar atmosphere for 2 hours. Obtain a transition metal-noble metal dual alloy catalyst, such as Figure 3a TEM results of the catalyst and Figure 3b The particle size distribution results show that the size of the main active sites in the catalyst is 4.3 nm.

[0064] One application of this embodiment is: 50 mg of the catalyst obtained in this embodiment is used to catalytically oxidize and remove hydrogen from a mixed gas of oxygen, nitrogen and hydrogen. The hydrogen concentration is 2000 ppm, the reaction temperature is 50°C, and the reaction time space velocity is 48000 mL·g -1 ·h -1 The space velocity was 1.5 ℃ and the stable hydrogen oxidation removal rate was 99.7%.

[0065] Example 4

[0066] Embodiment 4 of the present invention comprises the following steps:

[0067] Step a4, 0.5 mL of 0.09 M ethylenediamine coordinated Zn transition metal solution, 0.5 mL of 0.09 M ethylenediamine coordinated Pt noble metal solution and 7.5 g of deionized water were uniformly mixed by magnetic stirring for 30 min. Then 6.5 g of template agent tetrapropylammonium hydroxide and 4.2 g of silicon source tetraethoxysilane solution were added to the mixed solution, and magnetic stirring was performed for 6 h.

[0068] Step b4, transfer the mixed solution to a reactor, hydrotherm at 170°C, and react for 72 hours. Use deionized water for repeated centrifugation at a centrifugal speed of 8000rpm, centrifugal washing for 60 minutes, and finally wash until the pH is neutral. Dry the centrifuged catalyst at 80°C for 12 hours. Calcine the obtained powder material at 550°C in an air atmosphere for 6 hours, and then reduce it at 400°C in a H2 / Ar atmosphere for 2 hours. Obtain a transition metal-noble metal dual alloy MFI type pure silicon molecular sieve catalyst, such as Figure 4a TEM results of the catalyst and Figure 4b The particle size distribution results show that the size of the main active site in the catalyst is 3.1 nm.

[0069] One application of this embodiment is: 50 mg of the catalyst obtained in this embodiment is used to catalytically oxidize and remove hydrogen from a mixed gas of oxygen, nitrogen and hydrogen. The hydrogen concentration is 2000 ppm, the reaction temperature is 50°C, and the reaction time space velocity is 48000 mL·g -1 ·h -1 The space velocity was 1.53°, and a stable hydrogen oxidation removal efficiency of 78.8% was obtained.

[0070] Example 5

[0071] Step a5, 0.5 mL of 0.09 M ethylenediamine coordinated Mn transition metal solution, 0.5 mL of 0.09 M ethylenediamine coordinated Pt noble metal solution and 7.5 g of deionized water were uniformly mixed by magnetic stirring for 30 min. Then 6.5 g of template agent tetrapropylammonium hydroxide and 4.2 g of silicon source tetraethoxysilane solution were added to the mixed solution, and magnetic stirring was performed for 6 h.

[0072] Step b5, transfer the solution obtained by magnetic stirring to a reactor, hydrothermally heat at 170°C, and react for 72 hours. Use deionized water for repeated centrifugation, the centrifugal speed is 8000rpm, the centrifugal washing time is 60min, and finally wash until the pH is neutral. Dry the centrifuged catalyst at 80°C for 12h. Calcine the obtained powder material at 550°C in an air atmosphere for 6h, and then reduce it at 400°C in a H2 / Ar atmosphere for 2h. Obtain a transition metal-noble metal dual alloy MFI type pure silicon molecular sieve catalyst, such as Figure 5a TEM results of the catalyst and Figure 5bThe particle size distribution results show that the size of the main active sites in the catalyst is 3.2nm.

[0073] One application of this embodiment is: 50 mg of the catalyst obtained in this embodiment is used to catalytically oxidize and remove hydrogen from a mixed gas of oxygen, nitrogen and hydrogen. The hydrogen concentration is 2000 ppm, the reaction temperature is 50°C, and the reaction time space velocity is 48000 mL·g -1 ·h -1 The space velocity was 1.5 ℃ and the stable hydrogen oxidation removal rate was 99.8%.

[0074] Example 6

[0075] Embodiment 6 of the present invention further comprises the step of subjecting the powdered catalyst to a molding process to obtain a regularized catalyst. The specific steps of Embodiment 6 are as follows:

[0076] Step a6, 0.5 mL of 0.09 M ethylenediamine-coordinated Cu transition metal solution, 0.5 mL of 0.09 M ethylenediamine-coordinated Pt noble metal solution and 7.5 g of deionized water were uniformly mixed by magnetic stirring for 30 min. Then 6.5 g of template agent tetrapropylammonium hydroxide and 4.2 g of silicon source tetraethoxysilane solution were added to the mixed solution, and magnetic stirring was performed for 6 h.

[0077] Step b6, transfer the mixed solution to a reactor, hydrotherm at 170°C, and react for 72 hours. Use deionized water for repeated centrifugation, the centrifugal speed is 8000rpm, the centrifugal washing time is 60 minutes, and finally wash until the pH is neutral. Dry the centrifuged catalyst at 80°C for 12 hours. Calcine the obtained powder material at 550°C in an air atmosphere for 6 hours, and then reduce it at 400°C in a H2 / Ar atmosphere for 2 hours. Obtain a powdered transition metal-noble metal dual alloy MFI type pure silicon molecular sieve catalyst.

[0078] Step c6, add 1g of powdered catalyst to a mixed solution of sodium alginate and deionized water in a molar ratio of 1:300. After uniform mixing, the mixed solution is placed in a glass template mold with an outer diameter of 13mm and an inner diameter of 10mm. The catalyst-containing solution is cooled by liquid nitrogen and left to stand in the air for 12 hours before removing the mold. The resulting regularized catalyst is then freeze-dried at -30°C for 12 hours to finally obtain a regularized catalyst that follows the shape of the mold.

[0079] One application of this embodiment is to use the regularized catalyst obtained in this embodiment to catalytically oxidize and remove hydrogen from a mixed gas of oxygen, nitrogen and hydrogen. The hydrogen concentration is 2000 ppm, the reaction temperature is 50°C, and the reaction time space velocity is 12000 mL·g -1 ·h -1The space velocity was 1.5 ℃ and the stable hydrogen oxidation removal rate was 99.9%.

[0080] The restart performance of the structured catalyst was tested at a hydrogen concentration of 2000 ppm, a reaction temperature of 50 °C, and a reaction time space velocity of 12000 mL g -1 ·h -1 Under the space velocity condition, the structured catalyst can still maintain a stable hydrogen oxidation removal rate of 99% after multiple restart performance tests (cumulative time 30 days). Figure 6 shown.

[0081] Advantages of the present invention: The transition metal-noble metal dual alloy catalyst prepared by the present invention can be used for the catalytic oxidation and efficient removal of tritium-containing exhaust gas in tritium-related systems, and is particularly suitable for the deep oxidation and removal of low-concentration hydrogen isotope gas under low temperature conditions.

[0082] Example 7

[0083] This embodiment discloses a centrifugal cleaning device, which can be used for the centrifugal cleaning of embodiments 1 to 6. Figure 7 to Figure 12 As shown, the centrifugal cleaning device comprises:

[0084] The cylinder 1 has a cleaning chamber 11 with an upper opening and a mounting chamber 13 located below the cleaning chamber 11. The cleaning chamber 11 and the mounting chamber 13 are separated by a bottom plate 12. The side wall of the bottom plate 12 or the mounting chamber 13 has a drain port 14.

[0085] The driving member 2 is rotatably mounted on the cylinder 1, the upper end of the driving member 2 is located at the bottom of the cleaning chamber 11, and the lower end of the driving member 2 is located in the mounting chamber 13;

[0086] The driving motor 3 is located in the mounting cavity 13 and is used to drive the driving member 2 to rotate;

[0087] The container 4 is used to contain the objects to be cleaned. The container 4 includes a cylindrical screen 41 and a reinforcing sleeve 42 respectively fixed to the upper and lower ends of the cylindrical screen 41. The side wall and the bottom wall of the cylindrical screen 41 are both mesh structures. The reinforcing sleeve 42 at the lower end of the container 4 is used to seal the outer sleeve on the upper end of the driving member 2. A rotating clamping structure is provided between the reinforcing sleeve 42 and the driving member 2. When the motor drives the driving member 2 to rotate, the container 4 can be driven to rotate synchronously.

[0088] A first water pipe 51, which passes through the driving member 2 in a sealed manner and is used to inject water into the space formed by the driving member 2 and the receiving member 4. The driving member 2 can rotate relative to the first water pipe 51;

[0089] A water pump 52 is installed on the first water pipe 51;

[0090] A second water pipe 53, one end of which is connected to the drain port 14, and is used to drain the water in the installation cavity 13;

[0091] A cover 6 is detachably mounted on the upper end of the cylinder 1 and is used to cover the opening of the cleaning chamber 11;

[0092] The rotating plug 61 is rotatably mounted on the side of the cover 6 facing the cleaning chamber 11 through a bearing. The rotating plug 61 is used for sealing the reinforcing sleeve 42 provided on the upper end of the receiving member 4. When working, the rotating axes of the rotating plug 61, the receiving member 4 and the driving member 2 coincide with each other.

[0093] The pH detection sensor 7 is arranged in the installation cavity 13 and is used to detect the pH value of the liquid in the cylinder 1.

[0094] The portion of the driving member 2 located in the installation cavity 13 is provided with an L-shaped positioning portion 22, and the positioning portion 22 has an anti-slip groove 221; the outer wall of the reinforcing sleeve 42 at the lower end of the accommodating member 4 is fixed with a connecting portion 421, and the connecting portion 421 is used to be inserted into the space formed by the positioning portion 22 by rotation, and the connecting portion 421 has a protrusion 422, and the protrusion 422 is used to be inserted into the anti-slip groove 221. The accommodating member 4 can be taken out from the cylinder 1, as shown in FIG. Fig.11 As shown, it is the installed state. When it needs to be taken out, the receiving member 4 is rotated counterclockwise to make the protrusion 422 disengage from the anti-slip groove 221, and finally the connecting portion 421 is disengaged from the positioning portion 22, and then the receiving member 4 is moved up to be taken out. When installing, the receiving sleeve is first placed on the upper end of the driving member 2, and the connecting portion 421 is staggered with the positioning portion 22, and then the receiving member 4 is rotated clockwise to make the connecting portion 421 snap into the space formed by the positioning portion 22 until the protrusion 422 is embedded in the anti-slip groove 221. When the driving motor 3 is working, it is used to drive the driving member 2 to rotate counterclockwise, so that the receiving member 4 will not be separated from the positioning portion 22.

[0095] In order to prevent the driving member 2 from rotating together when the receiving member 4 is taken out, the driving member 2 can be generally pressed when taking out, so that the driving member 2 does not rotate. In actual use, preferably, the driving motor 3 is a self-locking motor.

[0096] like Figure 8 As shown, in this embodiment, the pH detection sensor 7 is located near the drain outlet 14, and can also be located inside the drain outlet 14 in actual use.

[0097] The centrifugal cleaning device of this embodiment further comprises a controller, and the driving motor 3 and the pH detection sensor 7 are both connected to the controller.

[0098] like Fig.11 As shown, the driving motor 3 drives the driving member 2 to rotate through a transmission structure such as gears.

[0099] like Fig.10As shown, the upper end of the driving member 2 has a first conical portion 21 that is smaller at the top and larger at the bottom. The first conical portion 21 is sealed with the reinforcing sleeve 42 at the lower end of the receiving member 4. Figure 8 As shown, the rotating plug 61 is a second tapered portion 611 that is larger at the top and smaller at the bottom. The second tapered portion 611 is sealed and matched with the reinforcing sleeve 42 at the upper end of the accommodating member 4.

[0100] like Figure 8 As shown, the upper end of the cylinder 1 has a positioning hole 15 , and the cover 6 has a positioning column 62 that matches the positioning hole 15 . The cylinder 1 and the cover 6 are connected to each other through the positioning hole 15 and the positioning column 62 .

[0101] Preferably, there is a magnetic adsorption structure between the cylinder 1 and the cover 6, for example, one of them has a first magnet, and the other has an iron-cobalt-nickel structure or a second magnet that is magnetically attracted to the first magnet.

[0102] The working principle of the centrifugal cleaning device of this embodiment is as follows: the material (solution) to be cleaned is placed in the container 4, the cover 6 is installed on the cylinder 1, the water pump 52 is working, and water (deionized water) is sprayed into the space formed by the first conical part 21 and the reinforcing sleeve 42 at the lower end of the container 4 through the first water pipe 51, and then the water enters the cylindrical screen 41 through the mesh bottom wall of the cylindrical screen 41. At the same time, the driving motor 3 is working to drive the driving member 2, the container 4 and the rotating plug 61 to rotate at a high speed. The water enters the cylindrical screen 41 and mixes with the material to be cleaned, and then is centrifugally thrown out. Through continuous centrifugal cleaning, the material to be cleaned is cleaned. Finally, when the pH value of the water detected by the pH detection sensor 7 is within the preset range (for example, neutral), the controller controls the driving motor 3 to stop rotating.

[0103] The centrifugal cleaning device of this embodiment can clean reliably and can automatically detect the pH value to achieve efficient cleaning.

[0104] The above description is only a preferred embodiment of the present invention, and does not limit the patent protection scope of the present invention. Any equivalent structural transformation made by using the contents of the present invention and the drawings, directly or indirectly used in other related technical fields, is also included in the protection scope of the present invention.

Claims

1. A method for preparing a transition metal-noble metal dual alloy catalyst, characterized in that: The steps include: Step a, mixing a transition metal source, a noble metal source and a molecular sieve precursor solution, and synthesizing a preliminary catalyst by a hydrothermal method; wherein the transition metal contained in the transition metal source is one or more of Fe, Co, Ni, Cu, Zn, Sn, and Mn oxides, and the noble metal contained in the noble metal source is one or more of Pt, Pd, Ru, and Rh metals; Step b, washing, drying, calcining and reducing the preliminary catalyst in sequence to obtain a powdery transition metal-noble metal dual alloy catalyst.

2. The method for preparing the transition metal-noble metal dual alloy catalyst according to claim 1, characterized in that: The transition metal source is a ligand-protected transition metal salt solution, and the noble metal source is an organic ligand-protected noble metal salt solution, wherein the ligand-protected solution is any one of ethylenediamine, dimethyldiethylamine, diethylenetriamine, and acetylacetone; the molar ratio between the transition metal salt and the organic ligand in the transition metal salt is 1:(15-35); the molar ratio between the noble metal salt and the organic ligand in the noble metal salt solution is 1:(10-30).

3. The method for preparing the transition metal-noble metal dual alloy catalyst according to claim 1, characterized in that: The molecular sieve precursor solution consists of a silicon source, a template agent and deionized water.

4. The method for preparing the transition metal-noble metal dual alloy catalyst according to claim 3, characterized in that: The silicon source is any one or more of tetraethoxysilane, methyltriethoxysilane, methyltripropoxysilane and trimethoxysilane; the template is any one of tetrapropylammonium hydroxide, tetrapropylammonium bromide and n-butylamine; and the molar ratio of the silicon source, the template and deionized water is 1:(0.3-0.7):(33-66).

5. The method for preparing the transition metal-noble metal dual alloy catalyst according to claim 1, characterized in that: The temperature of the hydrothermal synthesis is 120-170°C; the synthesis time is 24-96h.

6. The method for preparing the transition metal-noble metal dual alloy catalyst according to claim 1, characterized in that: The cleaning method in step b is centrifugation, the cleaning solvent is ethanol or deionized water, and the final washing is until the pH is neutral; The drying temperature is 50-100°C; the calcination temperature is 450-600°C; the reduction temperature is 350-550°C, and the reducing gas is at least one of H2 and Ar.

7. The method for preparing the transition metal-noble metal dual alloy catalyst according to claim 6, characterized in that: Cleaning is performed by a centrifugal cleaning device, the centrifugal cleaning device comprising: The cylinder body has a cleaning chamber with an upper opening and a mounting chamber located below the cleaning chamber, wherein the cleaning chamber and the mounting chamber are separated by a bottom plate, and the bottom plate or a side wall of the mounting chamber has a drainage port; A driving member is rotatably mounted on the cylinder, the upper end of the driving member is located at the bottom of the cleaning chamber, and the lower end of the driving member is located in the mounting chamber; A driving motor, located in the mounting cavity, for driving the driving member to rotate; A container for accommodating objects to be cleaned, the container comprising a cylindrical screen and reinforcing sleeves respectively fixed to the upper and lower ends of the cylindrical screen, the side wall and the bottom wall of the cylindrical screen being both mesh structures, the reinforcing sleeve at the lower end of the container being used to seal the outer sleeve on the upper end of the driving member, a rotating clamping structure being provided between the reinforcing sleeve and the driving member, and the container being able to rotate synchronously when the motor drives the driving member to rotate; a first water pipe, sealingly passing through the driving member and used for injecting water into the space formed by the driving member and the receiving member, wherein the driving member is rotatable relative to the first water pipe; a water pump, installed on the first water pipe; A second water pipe, one end of which is connected to the drain port and is used to drain the water in the installation cavity; A sealing cover, detachably mounted on the upper end of the cylinder, for covering the opening of the cleaning chamber; A rotating plug is rotatably mounted on the side of the cover facing the cleaning chamber through a bearing, and the rotating plug is used for sealing a reinforcing sleeve disposed on the upper end of the receiving member. When working, the rotating axes of the rotating plug, the receiving member and the driving member coincide with each other; The pH detection sensor is arranged in the installation cavity and is used to detect the pH value of the liquid in the cylinder.

8. The method for preparing the transition metal-noble metal dual alloy catalyst according to claim 1, characterized in that: The preparation method further comprises step c, forming the powdery transition metal-noble metal dual alloy catalyst, the specific method being: The powdered transition metal-noble metal dual alloy catalyst obtained in step b is uniformly dispersed in a mixed solution of sodium alginate and deionized water, the mixed solution is poured into a mold, cooled with liquid nitrogen and allowed to stand in the air for a certain period of time, and the mold is removed; the obtained granular catalyst is freeze-dried to obtain a regularized transition metal-noble metal dual alloy catalyst that follows the shape of the mold.

9. The method for preparing the transition metal-noble metal dual alloy catalyst according to claim 8, characterized in that: The molar ratio of sodium alginate to deionized water is 1: (300-400); the glass template mold has an outer diameter of 5-30 mm and an inner diameter of 3-28 mm; the freeze-drying temperature is -40--10° C.; and the freeze-drying time is 12-24 hours.

10. A transition metal-noble metal dual alloy catalyst, characterized in that: Prepared by the preparation method of the transition metal-noble metal dual alloy catalyst according to any one of claims 1 to 9; The transition metal-noble metal dual alloy catalyst is based on weight, the transition metal loading is 0.1-2wt.%, the noble metal loading is 0.1-2wt.%, and the prepared molecular sieve is a pure silicon molecular sieve with hydrophobicity, and the types of the pure silicon molecular sieve include MFI, FAU, and CHA.