Waste rubber slurry, preparation method and application thereof, and waste rubber slurry gasified gas
Waste rubber slurry is prepared through carbonization modification and wet co-grinding, and converted into CO and H2 gas through gasification reaction, which solves the problem of resource waste and pollution in waste rubber products and realizes the resource utilization of waste rubber , harmless use.
Patent Information
- Application Number
- CN202411152518.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
The existing technology cannot effectively utilize waste rubber products, resulting in waste of resources and environmental pollution, polluted gases are generated during the incineration process, and the high-temperature regeneration process takes a long time and consumes a large amount of regeneration additives, making it impossible to achieve resource-based and harmless utilization of waste rubber.
Rubber carbon is obtained by carbonizing and modifying waste rubber products, and mixed with slurry and surfactant for wet co-grinding or grinding to prepare waste rubber slurry, which is converted into CO and H2 gasification gas through gasification reaction , realize resource-based and harmless use.
This method reduces the consumption of inorganic acids and regenerators, avoids environmental pollution, and completely decomposes toxic and harmful substances. The gasified gas can be used for the synthesis of other chemicals, realizing the resource utilization of waste rubber.
Smart Images

Figure CN119035229A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waste rubber resource processing, and specifically relates to a waste rubber slurry, a preparation method and application thereof, and waste rubber slurry gasification gas. Background Art
[0002] Rubber has excellent properties such as air resistance, anti-seepage, damping and shock absorption, and acid and alkali solvent resistance. It is an indispensable practical material in many fields such as industry, transportation, medical treatment, military and military industry. With the rapid development of the rubber industry and the large-scale use and replacement of rubber products, the amount of discarded rubber products has gradually increased, such as rubber tubes, waste tires, rubber shock pads, scraps and unqualified waste generated in the production process of rubber products. Rubber has a stable structure, so waste rubber products are difficult to degrade under natural conditions, which will cause environmental pollution problems.
[0003] At present, the main treatment methods for rubber product waste include landfill, stacking, incineration, rubber powder filling and recycled rubber, among which landfill and stacking treatment will cause waste of resources and environmental pollution; incineration and heat energy utilization will produce a large amount of polluting gases; the preparation of rubber powder and recycled rubber industry generally adopts high-temperature regeneration technology, and the production process requires the addition of a large amount of regeneration additives. The regeneration temperature is high and the time is long. Finally, refining treatment is required. The production process will also produce a large amount of polluting gases. At the same time, recycled rubber cannot be used in large quantities as rubber filling materials.
[0004] In summary, the existing treatment methods cannot achieve the resource recovery and harmless utilization of rubber product waste, and there is an urgent need for a method that can achieve the resource recovery and harmless utilization of waste rubber products. Summary of the invention
[0005] The purpose of the present invention is to provide a waste rubber slurry, a preparation method and application thereof, and waste rubber slurry gasification gas. The preparation method of the waste rubber slurry provided by the present invention realizes the resource recovery and harmless utilization of waste rubber products.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing waste rubber slurry, comprising the following steps:
[0008] Carbonizing and modifying the waste rubber products to obtain waste rubber charcoal;
[0009] The waste rubber carbon, slurry and surfactant are mixed and wet-grinded to obtain waste rubber slurry, or the waste rubber carbon is ground and then mixed with slurry and surfactant to obtain waste rubber slurry; the slurry includes water and / or organic waste liquid.
[0010] Preferably, the calorific value of the waste rubber charcoal is >12000 j / g and the water content is <20 wt%.
[0011] Preferably, the carbonization modification temperature is 200-600°C and the time is 0.2-5h;
[0012] The carbonization modification is carried out under anaerobic conditions; the oxygen content of the anaerobic conditions is ≤1VOL%;
[0013] The carbonization modification also produces carbonized gas, which can be used as fuel.
[0014] Preferably, the surfactant includes one or more of lignin sulfonate surfactants, naphthalene sulfonate surfactants, sulfonated humate surfactants and polyolefin surfactants.
[0015] Preferably, the mass ratio of the slurry to the surfactant is 100:0.2-5; the ratio of the mass of the waste rubber charcoal to the total mass of the slurry and the surfactant is 10:4-90.
[0016] Preferably, the organic waste liquid includes non-aqueous organic waste liquid and / or organic waste water; the calorific value of the non-aqueous organic waste liquid is >10000 J / g; the calorific value of the organic waste water is >800 J / g.
[0017] The present invention provides waste rubber slurry prepared by the preparation method described in the above technical scheme, wherein the waste rubber slurry has a solid content of 10 to 70 wt%, a calorific value of >10000 j / g, a viscosity of 200 to 1600 mPa·s, a fluidity of 5 to 40 s, an ash content of 2 to 25 wt%, and a 24-hour static water separation rate of 0.2 to 2%.
[0018] The present invention provides the application of the waste rubber slurry described in the above technical solution in the resource utilization of waste rubber.
[0019] The present invention provides a waste rubber slurry gasification gas, which is obtained by gasifying the waste rubber slurry described in the above technical solution;
[0020] The waste rubber slurry gasification gas includes CO and H2.
[0021] Preferably, the gasification temperature is 1100-1750° C. and the pressure is 0.2-10 MPa.
[0022] The method for preparing waste rubber slurry provided by the present invention is to carbonize and modify waste rubber products, and the obtained rubber charcoal has strong grindability and can be used as a raw material for preparing waste rubber slurry. Compared with the methods of treating waste rubber products such as incineration and recycled rubber, the present invention mixes the waste rubber charcoal, slurry and surfactant, and performs wet co-grinding, or grinds the waste rubber charcoal and mixes it with slurry and surfactant to prepare waste rubber slurry, which makes full use of the organic components in the waste rubber products, while reducing the consumption of inorganic acid and regeneration agent, avoiding environmental pollution, and being green and environmentally friendly; the carbonized and modified waste rubber charcoal is mixed with the slurry to prepare a gasification gas (effective gas) mainly composed of CO and H2, which can completely decompose the toxic and harmful substances in the organic slurry without causing secondary pollution, and the gasification gas can be used for the synthesis of other chemicals, realizing the resource and harmless utilization of waste rubber products. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a flow chart of preparing gasification gas from waste rubber slurry in Example 1;
[0024] Figure 2 This is a flow chart of preparing gasification gas for waste rubber slurry in Example 4. DETAILED DESCRIPTION
[0025] The present invention provides a method for preparing waste rubber slurry, comprising the following steps:
[0026] Carbonizing and modifying the waste rubber products to obtain waste rubber charcoal;
[0027] The waste rubber carbon, slurry and surfactant are mixed and wet-grinded to obtain waste rubber slurry, or the waste rubber carbon is ground and then mixed with slurry and surfactant to obtain waste rubber slurry; the slurry includes water and / or organic waste liquid.
[0028] In the present invention, unless otherwise specified, the reagents used are commercially available products well known to those skilled in the art.
[0029] The invention carbonizes and modifies waste rubber products to obtain waste rubber charcoal. In the present invention, the waste rubber products preferably include one or more of waste rubber pipes, waste tires and waste rubber shock pads; the temperature of the carbonization modification is preferably 200-600°C, more preferably 250-550°C, further preferably 350-480°C, specifically preferably 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 480°C, 500°C, 550°C or 600°C; the time of the carbonization modification is preferably 0.2-5h, more preferably 0.5-4h, further preferably 1-3.5h, specifically preferably 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h; the carbonization modification is preferably carried out under anaerobic conditions; the oxygen content of the anaerobic conditions is preferably ≤1VOL%, more preferably 0.2-0.8VOL%, and most preferably 0.4-0.6VOL%. In the present invention, the calorific value of the waste rubber charcoal is preferably ≥12000 j / g, more preferably 13000-30000 j / g, and most preferably 20000-26000 j / g; the moisture content of the waste rubber charcoal is preferably <20wt%, more preferably 15-19wt%, and most preferably 16-18wt%.
[0030] In the present invention, the carbonization modification preferably also produces carbonization gas. In the present invention, waste rubber products are carbonized under anaerobic conditions, and the carbonization gas generated during the carbonization modification process is collected and processed for recycling as fuel, and the remaining residue is waste rubber charcoal. The obtained waste rubber charcoal has strong grindability, low moisture content, and high calorific value, and can be used as a raw material for preparing waste rubber slurry.
[0031] After obtaining the waste rubber carbon, the present invention mixes the waste rubber carbon, a slurry and a surfactant, and performs wet co-grinding to obtain waste rubber slurry.
[0032] In the present invention, the slurry comprises water and / or organic waste liquid; the organic waste liquid preferably comprises non-aqueous organic waste liquid and / or organic waste water; the calorific value of the non-aqueous organic waste liquid is preferably>10000j / g, more preferably 12000j / g-18000j / g, further preferably 14000-16000j / g, specifically preferably 11000j / g, 11514j / g, 12000j / g, 12850j / g, 13244j / g , 14000J / g, 16000J / g, 18000J / g, 20000J / g or 22000J / g; the calorific value of the organic wastewater is preferably>800J / g, more preferably 2200-3000J / g, further preferably 2500-2800J / g, specifically preferably 1000J / g, 1600J / g, 2200J / g, 2800J / g, 3000J / g, 3600J / g or 4200J / g. The present invention uses organic waste liquid with higher calorific value, which is conducive to the gasification of the obtained waste rubber slurry.
[0033] In the present invention, the surfactant preferably includes one or more of lignin sulfonate surfactants, naphthalene sulfonate surfactants, sulfonated humate surfactants and polyolefin surfactants; the lignin sulfonate surfactant preferably includes one or more of sodium lignin sulfonate, ammonium lignin sulfonate and potassium lignin sulfonate; the naphthalene sulfonate surfactant preferably includes sodium monoalkyl naphthalene sulfonate and / or sodium dialkyl naphthalene sulfonate; the sulfonated humate surfactant preferably includes potassium sulfonated humate and / or sodium sulfonated humate; the polyolefin surfactant preferably includes tert-butyl octanoate and / or tert-butyl peroxide. The present invention uses a surfactant with hydrophilic and lipophilic properties, which is beneficial to improving the hydrophilicity of waste rubber charcoal, improving slurrying properties, and improving the stability of waste rubber slurry.
[0034] In the present invention, the mass ratio of the slurry to the surfactant is preferably 100:0.2-5, more preferably 100:0.2-3, further preferably 100:1-2, specifically preferably 100:0.2, 100:0.3, 100:0.4, 100:0.5, 100:1, 100:1.5, 100:2, 100:2.5, 100:3, 100:3.5, 100:4, 100:4.5 or 100:5; the mass ratio of the waste rubber charcoal to the total mass of the slurry and the surfactant is preferably 10:4-90, more preferably 10:6-70, further preferably 10:7-25, specifically preferably 10:4, 10:6, 10:8, 10:10, 10:15, 10:20, 10:30, 10:40 or 10:90.
[0035] In the present invention, the slurry and the surfactant are preferably used in the form of a mixed solution of the slurry and the surfactant; the raw materials for preparing the mixed solution preferably also include a pH adjuster; the pH adjuster preferably includes an inorganic base and / or an alkaline salt; the inorganic base preferably includes potassium hydroxide and / or sodium hydroxide; the alkaline salt preferably includes ammonium bicarbonate and / or sodium bicarbonate. In the present invention, the pH value of the mixed solution is preferably 5 to 8, more preferably 6 to 7, further preferably 6.5 to 6.8, and specifically preferably 5, 5.5, 6, 6.5, 7, 7.5 or 8. The present invention can reduce damage to gasifier furnace bricks and pipelines during the gasification process by adjusting the pH of the mixed solution to neutral or weakly acidic.
[0036] In the present invention, the wet co-grinding time is preferably 0.2 to 1 h, more preferably 0.5 to 1 h, and most preferably 0.8 to 1 h. In the present invention, the proportion of particles with a mesh size of >200 mesh in the powder obtained by the wet co-grinding is preferably 40 to 70%, more preferably 45 to 65%, and most preferably 50 to 60%, the proportion of particles with a mesh size of >100 mesh is preferably 75 to 90%, more preferably 80 to 88%, and most preferably 82 to 85%, and the proportion of particles with a mesh size of >14 mesh is preferably 98 to 100%, and more preferably 99 to 100%.
[0037] After obtaining the waste rubber charcoal, the present invention grinds the waste rubber charcoal and mixes it with a slurry and a surfactant to obtain a waste rubber slurry; the slurry includes water and / or organic waste liquid. In the present invention, the types of the slurrying agent and the surfactant, the amounts of the waste rubber charcoal, the slurry and the surfactant are preferably the same as those described above and are not repeated here. In the present invention, the grinding time is preferably 0.2 to 1h, more preferably 0.4 to 0.8h, and most preferably 0.6 to 0.7h. In the present invention, the proportion of the powder obtained by grinding with a particle size of >200 mesh is preferably 40 to 70%, more preferably 45 to 65%, and most preferably 50 to 60%.
[0038] The present invention provides a waste rubber slurry prepared by the preparation method of the above technical scheme, wherein the solid content of the waste rubber slurry is 10-70wt%, more preferably 12-63wt%, and specifically preferably 10wt%, 20wt%, 25wt%, 30wt%, 40wt%, 50wt%, 55wt%, 62wt% or 70wt%; the calorific value is>10000j / g, preferably 14000-19000j / g, and more preferably 16000-18000j / g; the viscosity is 200-1600mPa·s, preferably 400-800mPa·s, more preferably 600-700mPa·s, and specifically preferably 200mPa·s, 400mPa·s, 600mPa·s, 800mPa·s, 1000mPa·s, 1200mPa·s, 1400mPa·s or 1600mPa·s; fluidity (the time for a quantitative material to pass through a mold) is 5 to 40s, preferably 5 to 25s, more preferably 6 to 20s, and specifically preferably 5s, 6s, 8s, 10s, 15s, 20s, 25s, 30s, 35s, and 40s; the ash content is 2 to 25wt%, preferably 5 to 20wt%, more preferably 10 to 15wt%, and specifically preferably 2wt%, 4wt%, 8wt%, 10wt%, 12wt%, 15wt%, 17wt%, 19wt%, 21wt%, 23wt% or 25wt%; the 24h static water separation rate is 0.2 to 2%, preferably 0.4 to 1.0%, more preferably 0.6 to 0.8%, and specifically preferably 0.2%, 0.4%, 0.6%, 0.8%, 1.0%, 1.4%, 1.6%, 1.8% or 2.0%. The waste rubber slurry provided by the present invention has low 24h static water separation rate, good stability (a high water separation rate indicates that the slurry and waste liquid are separated and the sedimentation speed is fast), good fluidity, and avoids pipeline blockage caused by adhesion to the pipeline due to excessive viscosity.
[0039] The present invention provides the application of the waste rubber slurry described in the above technical solution in the resource utilization of waste rubber. The present invention makes full use of the organic components in the waste rubber products, while reducing the consumption of inorganic acid and regeneration agent, avoiding environmental pollution, and being green and environmentally friendly; the carbonized and modified waste rubber charcoal is mixed with the slurry to prepare the gasification gas mainly composed of CO and H2 through the gasification reaction, which can completely decompose the toxic and harmful substances in the organic slurry without generating secondary pollution, and the gasification gas can be used for the synthesis of other chemicals, thus realizing the resource utilization and harmless utilization of waste rubber products.
[0040] The present invention provides a waste rubber slurry gasification gas obtained by gasifying the waste rubber slurry described in the above technical solution; the waste rubber slurry gasification gas includes CO and H2. In the present invention, the total content of CO and H2 in the waste rubber slurry gasification gas is preferably 50-88VOL%, more preferably 73-83VOL%, and most preferably 75-81VOL%.
[0041] In the present invention, the temperature is 1100-1750°C, more preferably 1150-1450°C, and most preferably 1200-1400°C; the pressure of the gasification is preferably 0.2-10MPa; more preferably 0.5-5MPa, and most preferably 1-2MPa. In the present invention, the gasification is preferably carried out in an oxygen-containing atmosphere; the concentration of oxygen in the oxygen-containing atmosphere is preferably ≥99.5v / v%, more preferably 99.5-100v / v%, and most preferably 99.7-99.8v / v%.
[0042] After the gasification is completed, the present invention preferably further comprises purifying the mixed gas obtained by the gasification. In the present invention, the mixed gas preferably comprises CO, CO2, H2, N2 and CH4. The present invention gasifies the waste rubber slurry in an oxygen-containing atmosphere (semi-redox), which can completely decompose the organic matter in the rubber product waste without generating secondary pollution. The obtained mixed gas containing CO, CO2, H2, N2 and CH4 is purified to prepare a gasification gas mainly composed of CO and H2, thereby realizing the resource and harmless utilization of waste rubber products. After the rubber slurry is mixed with oxygen and sprayed into the gasifier, the water content quickly turns into water vapor, and the rubber powder undergoes dry distillation and thermal cracking. The powder turns into coke, and due to the high oxygen concentration in this area, the volatile matter is quickly and completely burned at high temperature, while releasing a large amount of heat. On the other hand, it undergoes a combustion reaction with the remaining oxygen to generate gases such as CO2 and CO, and releases heat. On the other hand, coal coke undergoes a gasification reaction with water vapor and CO2 to generate H2 and CO. In the gas phase, H2, CO and residual O2 undergo combustion reaction to release heat. In order to further illustrate the present invention, the following is a detailed description of a waste rubber slurry, a preparation method and application thereof, and a waste rubber slurry gasification gas provided by the present invention in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0043] In all embodiments of the present invention, the atomizer used is a three-channel atomizer, the central channel is oxygen, the middle channel is waste rubber slurry, and the outer channel is oxygen.
[0044] Example 1
[0045] Figure 1 This is a flow chart of preparing the gasification gas of waste rubber slurry in Example 1, and the steps are as follows:
[0046] Waste tires were added into a carbonization reactor and carbonized at 450°C for 1 hour under the conditions of anoxicity (oxygen content of 0.8VOL%) to obtain grindable waste rubber charcoal, which was then discharged from the carbonization reactor via a screw conveyor for standby use. The calorific value of the waste rubber charcoal was 24385 j / g and the water content was 12 wt%.
[0047] 20 t of organic waste liquid with a calorific value of 12000 j / g and 0.2 t of sodium lignin sulfonate were uniformly mixed, and the pH value was adjusted to 6.5 with sodium bicarbonate to obtain a pre-treated liquid.
[0048] 17 tons of waste rubber charcoal and 20.4 tons of pretreatment liquid were added to the pulping device in sequence, and wet co-grinding pulping was carried out for 1 hour to make the waste rubber charcoal and the pretreatment liquid react to obtain waste rubber slurry.
[0049] The obtained waste rubber slurry and a mixed atmosphere containing 99.6 v / v% oxygen are respectively sprayed into a high-temperature melting reactor through an atomizer, and a gasification reaction is carried out at a temperature of 1200°C and a pressure of 1.2 MPa to obtain a gaseous product and liquid slag; the gaseous product is washed to obtain a waste rubber slurry gasification gas with a CO and H2 volume content of 75%, and the liquid slag is water-quenched to obtain a glassy slag, which is used in the construction industry after being tested and identified as qualified.
[0050] Example 2
[0051] The waste rubber tube was added into the carbonization reactor and carbonized at 480°C for 4.5 hours under the condition of lack of oxygen (oxygen content was 0.5VOL%) to obtain grindable waste rubber charcoal, which was discharged from the carbonization reactor through a screw conveyor for standby use. The calorific value of the waste rubber charcoal was 23542j / g and the water content was 16wt%.
[0052] 3.94t of organic waste liquid with a calorific value of 12850j / g and 0.06t of potassium lignin sulfonate were uniformly mixed, and the pH value was adjusted to 6.8 with sodium bicarbonate to obtain a pre-treated liquid.
[0053] 4 tons of waste rubber charcoal and 4 tons of pretreatment liquid were added into the pulping device in sequence, and wet co-grinding pulping was carried out for 1 hour to make the waste rubber charcoal and the pretreatment liquid react to obtain waste rubber slurry.
[0054] The obtained waste rubber slurry and the mixed atmosphere containing 99.5v / v% oxygen are respectively sprayed into a high-temperature melting reactor through an atomizer, and a gasification reaction is carried out at a temperature of 1250°C and a pressure of 1.3MPa to obtain a gaseous product and liquid slag; the gaseous product is washed to obtain a waste rubber slurry gasification gas with a CO and H2 volume content of 81%, and the liquid slag is water-quenched to obtain a glassy slag, which is used in the construction industry after being tested and identified as qualified.
[0055] Example 3
[0056] Waste tires were added into a carbonization reactor and carbonized at 480°C for 5 hours under the conditions of anoxicity (oxygen content of 0.6 VOL%) to obtain grindable waste rubber charcoal, which was then discharged from the carbonization reactor via a screw conveyor for standby use. The calorific value of the waste rubber charcoal was 26423 J / g and the water content was 15 wt%.
[0057] 10 t of water and 0.2 t of sodium lignin sulfonate were uniformly mixed, and the pH value was adjusted to 8 with sodium bicarbonate to obtain a pretreatment solution.
[0058] 12.75t of waste rubber charcoal and 10.2t of pretreatment liquid were sequentially added into the pulping device and wet co-grinded for 0.5h to make the waste rubber charcoal and the pretreatment liquid react to obtain waste rubber slurry.
[0059] The obtained waste rubber slurry and the mixed atmosphere containing 99.8v / v% oxygen are respectively sprayed into a high-temperature melting reactor through an atomizer, and a gasification reaction is carried out at a temperature of 1250°C and a pressure of 1.3MPa to obtain a gaseous product and liquid slag; the gaseous product is washed to obtain a waste rubber slurry gasification gas with a CO and H2 volume content of 73%, and the liquid slag is water-quenched to obtain a glassy slag, which is used in the construction industry after being tested and identified as qualified.
[0060] Example 4
[0061] Figure 2 This is a flow chart of preparing the gasification gas of waste rubber slurry in Example 4, and the steps are as follows:
[0062] The waste rubber shock-absorbing pad was added into a carbonization reactor, and carbonized for 2.5 hours at 550°C under the conditions of anoxic (oxygen content of 0.2VOL%) to obtain grindable waste rubber charcoal, which was discharged from the carbonization reactor through a screw conveyor and ground to obtain waste rubber charcoal powder for use. The calorific value of the waste rubber charcoal powder was 22894j / g, and the water content was 18wt%.
[0063] 31.84t of organic waste liquid with a calorific value of 13244j / g and 0.16t of sodium sulfonated humate were uniformly mixed, and the pH value was adjusted to 7.2 with sodium bicarbonate to obtain a pre-treated liquid.
[0064] 40 tons of waste rubber carbon powder and 32 tons of pretreatment liquid were added into the pulping device in sequence, mixed and stirred for 1 hour to make the waste rubber carbon and the pretreatment liquid react to obtain waste rubber slurry.
[0065] The obtained waste rubber slurry and the mixed atmosphere containing 99.6v / v% oxygen are respectively sprayed into a high-temperature melting reaction furnace through an atomizer, and a gasification reaction is carried out at a temperature of 1350°C and a pressure of 1.35MPa to obtain a gaseous product and liquid slag; the gaseous product is washed to obtain a waste rubber slurry gasification gas with a CO and H2 volume content of 85%, and the liquid slag is water-quenched to obtain a glassy slag, which is used in the construction industry after being tested and identified as qualified.
[0066] Example 5
[0067] The waste rubber shock-absorbing pad was added into a carbonization reactor, and carbonized for 3 hours at 350°C under the conditions of lack of oxygen (oxygen content is 0.6VOL%) to obtain grindable waste rubber charcoal, which was discharged from the carbonization reactor through a screw conveyor and ground to obtain waste rubber charcoal powder for use. The calorific value of the waste rubber charcoal powder was 24322j / g and the water content was 16wt%.
[0068] 31.53 t of organic waste liquid with a calorific value of 11514 j / g and 0.47 t of potassium polyolefin sulfonate were uniformly mixed, and the pH value was adjusted to 7.8 with sodium bicarbonate to obtain a pre-treated liquid.
[0069] 20 tons of waste rubber carbon powder and 32 tons of pretreatment liquid were added into the pulping device in sequence, mixed and stirred for 1 hour to make the waste rubber carbon and the pretreatment liquid react to obtain waste rubber slurry.
[0070] The obtained waste rubber slurry and the mixed atmosphere containing 99.7v / v% oxygen are respectively sprayed into a high-temperature melting reaction furnace through an atomizer, and a gasification reaction is carried out at a temperature of 1150°C and a pressure of 1.3MPa to obtain a gaseous product and liquid slag; the gaseous product is washed to obtain a waste rubber slurry gasification gas with a CO and H2 volume content of 79%, and the liquid slag is water-quenched to obtain a glassy slag, which is used in the construction industry after being tested and identified as qualified.
[0071] The calorific value, solid content, viscosity, fluidity, ash content and 24h static water separation rate of the waste rubber slurry prepared in Examples 1 to 5 were tested. The results are shown in Table 1. The test method is as follows:
[0072] Calorific value: Take 0.2-0.5g of rubber slurry and put it in an oxygen bomb. The sample is burned in the oxygen bomb filled with excess oxygen and the heat released by combustion is tested in j / g.
[0073] Solid content: After the rubber slurry is fully stirred, 3 g of the sample is weighed into a weighing bottle and dried at 110°C until the mass is constant. The mass fraction of the dried sample mass to the original sample mass is taken as the rubber slurry concentration, in %.
[0074] Viscosity: Rubber slurry is placed in the outer cylinder of the coaxial cylinder rotation viscometer, and the inner cylinder is heated at a shear rate of 100 s at 26°C. -1 The cylinder rotates under the conditions and the viscous torque it is subjected to during the rotation is measured, thereby calculating the viscosity in millipascal seconds (mPa·s).
[0075] Fluidity: After the rubber slurry is fully stirred, 200 mL of the sample is weighed into a funnel mold (the upper part is cylindrical and the lower part is a glass tube with a diameter of 1 cm). The outlet is sealed with a rubber stopper. At the beginning of the test, the rubber stopper is removed and the time for all the rubber slurry to flow out of the glass tube is recorded in seconds.
[0076] Ash content: After the rubber slurry is fully stirred, 1 g of the sample is weighed into an ash dish, placed in a muffle furnace, and burned at 810°C to constant weight. The percentage of the residue in the mass of the rubber slurry is taken as the ash content of the rubber slurry, expressed in percentage (%).
[0077] Water absorption rate: Stir the rubber slurry sample thoroughly to make it uniform, pour the stirred rubber slurry into a 200mL measuring cylinder, record the rubber slurry liquid level (h) in the measuring cylinder and seal it, and record the liquid level of the precipitated water in the measuring cylinder (h1) after standing at room temperature for 24 hours. 24h static water absorption rate (%) = h1 / h*100%.
[0078] Table 1 Performance test results of waste rubber slurry prepared in Examples 1 to 5
[0079] Serial number <![CDATA[Calorific value / J / g -1 > Solid content / % Viscosity / mPa·s Liquidity / s Ash / % 24h static water separation rate / % Example 1 17625 45.5 652 7 13.2 0.3 Example 2 18236 49.96 704 8 14.3 0.3 Example 3 14679 55.6 722 8 14.6 0.7 Example 4 18617 56.84 1240 18 17.6 0.8 Example 5 16485 39.06 488 6 11.7 0.7
[0080] As can be seen from Table 1, the waste rubber slurry prepared by the present invention has a low water separation rate and good fluidity, and the data such as solid content, calorific value, viscosity, fluidity, ash content, etc. all meet the use indicators.
[0081] Table 2 Composition of gasified gas from waste rubber slurry prepared in Examples 1 to 5
[0082] Content / VOL% <![CDATA[CO2]]> <![CDATA[O2]]> CO <![CDATA[H2]]> <![CDATA[CH4]]> <![CDATA[N2]]> Example 1 21.2 0.1 45.5 29.5 0.57 3.13 Example 2 16.5 0.1 48.3 32.7 0.35 2.05 Example 3 23.6 0.1 43.9 29.1 0.89 2.41 Example 4 13.4 0.1 51.4 33.6 0.27 1.23 Example 5 17.9 0.1 45.9 33.1 0.69 2.41
[0083] Table 2 is a table of gasification gas compositions of waste rubber slurry prepared in Examples 1 to 5. It can be seen from Table 2 that the waste rubber slurry provided by the present invention obtains gasification gas mainly composed of CO and H2 through gasification reaction, which can completely decompose toxic and harmful substances in the organic slurry without causing secondary pollution, thereby realizing the resource and harmless utilization of waste rubber products.
[0084] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing waste rubber slurry, characterized in that: The following steps are involved: Carbonizing and modifying the waste rubber products to obtain waste rubber charcoal; The waste rubber carbon, slurry and surfactant are mixed and wet-grinded to obtain waste rubber slurry, or the waste rubber carbon is ground and then mixed with slurry and surfactant to obtain waste rubber slurry; the slurry includes water and / or organic waste liquid.
2. The preparation method according to claim 1, characterized in that: The calorific value of the waste rubber charcoal is greater than 12000 j / g, and the moisture content is less than 20 wt%.
3. The preparation method according to claim 1 or 2, characterized in that: The carbonization modification temperature is 200-600°C and the time is 0.2-5h; The carbonization modification is carried out under anaerobic conditions; the oxygen content of the anaerobic conditions is ≤1VOL%; The carbonization modification also produces carbonized gas, which can be used as fuel.
4. The preparation method according to claim 1, characterized in that: The surfactant includes one or more of lignin sulfonate surfactants, naphthalene sulfonate surfactants, sulfonated humate surfactants and polyolefin surfactants.
5. The preparation method according to claim 1 or 4, characterized in that: The mass ratio of the slurry to the surfactant is 100:0.2-5; the mass ratio of the waste rubber charcoal to the total mass of the slurry and the surfactant is 10:4-90.
6. The preparation method according to claim 1, characterized in that: The organic waste liquid includes non-aqueous organic waste liquid and / or organic waste water; the calorific value of the non-aqueous organic waste liquid is greater than 10000 J / g; the calorific value of the organic waste water is greater than 800 J / g.
7. The waste rubber slurry obtained by the preparation method according to any one of claims 1 to 6, characterized in that: The waste rubber slurry has a solid content of 10-70wt%, a calorific value>10000j / g, a viscosity of 200-1600mPa·s, a fluidity of 5-40s, an ash content of 2-25wt%, and a 24h static water separation rate of 0.2-2%.
8. Use of the waste rubber slurry according to claim 7 in the resource utilization of waste rubber.
9. A waste rubber slurry gasification gas, characterized in that: Obtained by gasifying the waste rubber slurry as claimed in claim 7; The waste rubber slurry gasification gas includes CO and H2.
10. The waste rubber slurry gasification gas according to claim 9, characterized in that: The gasification temperature is 1100-1750° C. and the pressure is 0.2-10 MPa.
Citation Information
Patent Citations
Method for preparing activated carbon by utilizing waste tire rubber
CN101708841A
Spent activated carbon resource utilization method
CN108517226A
Coal gasification fine slag black water treatment method, modified slag and application of modified slag
CN118062939A
Process for oxygen pulping of lignocellulosic material and recovery of pulping chemicals
CN1340121A
Burning treatment method of waste tire
JP1994031262A