Alcohol-based binder as well as preparation method and use method thereof

Through the preparation and use of alcohol-based adhesives, the problems of insufficient bonding performance and poor compatibility in the prior art are solved, and efficient bonding and rapid curing of metal powders are achieved. It is suitable for the preparation of complex-shaped metal parts. Important application value.

CN119035538APending Publication Date: 2024-11-29KOCEL INTELLIGENT MACHINERY LIMITED
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411191262.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the existing metal adhesive spray 3D printing technology, insufficient bonding performance and poor compatibility with metal powders limit the preparation and application of complex shape metal parts.

Method used

Using alcohol-based binders, including polyvinylpyrrolidone, stabilizers and surfactants, prepared by specific mixing and stirring steps, combined with jet 3D printing technology, directional spraying and curing metal powders .

Benefits of technology

It achieves good fluidity and rapid curing properties of the binder, improves compatibility with metal powders, and is especially suitable for lightweight metal products, and has important aerospace and biomedical application value.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an alcohol-based binder which comprises the following components in parts by weight: 10-15 parts of polyvinylpyrrolidone, 5-10 parts of a stabilizer, 10-20 parts of a surfactant and 55-75 parts of a solvent. According to the alcohol-based binder disclosed by the invention, the polyvinylpyrrolidone is adopted as a base material to consolidate the metal powder, the surfactant can effectively improve the wettability of the binder on the surface of the metal powder, and the ethylene glycol monomethyl ether is used as a solvent to greatly reduce the surface tension of the binder; and by adding the stabilizer, the chemical uniformity and stability of the binder can be maintained. The alcohol-based binder disclosed by the invention has good flowability and rapid curing performance, has good compatibility with metal powder, especially titanium alloy metal powder, is particularly suitable for binder jet 3D printing of light metal products, and particularly has important application value in the fields of aerospace, biomedicine and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of additive manufacturing, and in particular to an alcohol-based binder and a preparation method and a use method thereof. Background Art

[0002] Metal binder jet 3D printing technology is an emerging metal 3D printing technology that uses a binder to bond metal powders and stack them layer by layer to form a complex metal structure. Metal binder jet 3D printing technology provides a new option for manufacturing complex shapes and customized metal parts. The development of low-energy, low-cost, and highly universal binder jet 3D printing technology can achieve the preparation of high-performance, large-size, complex-shaped metal parts, which is of great significance to broadening the application field of additive manufacturing.

[0003] In the process of binder jetting 3D printing, the selection of binder is crucial. The binder needs to have good fluidity, fast curing performance and good compatibility with metal powder. There are still some problems with the existing binders used in metal binder jetting 3D printing, such as insufficient bonding performance and poor compatibility with metal powder. These problems limit the development and application of binder jetting 3D printing metal technology. Therefore, it is of great significance to develop a new type of binder suitable for binder jetting 3D printing metal. Summary of the invention

[0004] Based on this, in order to solve the above technical problems, the present invention provides an alcohol-based binder suitable for binder jetting 3D printing of metals, and a preparation method and a use method thereof.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] An alcohol-based adhesive comprises, by weight, 10 to 15 parts of polyvinyl pyrrolidone, 5 to 10 parts of a stabilizer, 10 to 20 parts of a surfactant and 55 to 75 parts of a solvent.

[0007] Furthermore, the solvent is ethylene glycol monomethyl ether. Compared with other solvents, ethylene glycol monomethyl ether has the function of improving the wetting effect and viscosity in the bonding system of the present invention, and can better meet the parameter requirements of the print head nozzle jet printing. In addition, ethylene glycol monomethyl ether is volatile and has strong permeability as a solvent, which can appropriately increase the thickness of the printed layer and improve the printing efficiency.

[0008] Furthermore, the stabilizer is at least one of 2-pyrrolidone or ethylene acrylic acid, which can effectively improve the toughness, plasticity, strength and hardness of the printed product.

[0009] Furthermore, the surfactant is at least one of diethylene glycol, diethylene glycol and ethylene glycol butyl ether.

[0010] Furthermore, the molecular weight of the polyvinyl pyrrolidone is 40,000 to 60,000 g / mol, the viscosity is suitable and does not affect the degreasing efficiency of the printed product.

[0011] In a second aspect, the present application further provides a preparation method, which is applied to any of the above-mentioned alcohol-based binders, and the preparation method comprises the following steps:

[0012] S110, mixing the solvent and the surfactant, and stirring for 10 to 20 minutes;

[0013] S120, adding the stabilizer and stirring for 10 to 20 minutes;

[0014] S130, adding the polyvinyl pyrrolidone and stirring for 20 to 40 minutes.

[0015] It should be noted that each step in the preparation method of the alcohol-based binder disclosed in the present invention is carried out at room temperature without heating reaction.

[0016] In a third aspect, the present application also provides a method of use, which is applied to any of the alcohol-based binders described above, wherein the alcohol-based binder is used for binder jetting 3D printing of metal powders.

[0017] Furthermore, the method for using the alcohol-based binder comprises the following steps:

[0018] S210, importing the printing model into the 3D printer;

[0019] S220, the working box descends by one layer thickness, and the powder spreader spreads powder; the layer thickness is set to 20 to 80 microns;

[0020] S230, the print head sprays the binder onto the powder layer in a directional manner;

[0021] S240, repeating the step S220 and the step S230 until printing is completed.

[0022] Furthermore, after the step S240, the method further includes sequentially curing, degreasing and sintering the printed product;

[0023] In the curing step, the curing temperature is 150 to 200° C. and the curing time is 180 to 600 minutes;

[0024] In the degreasing step, the degreasing temperature is 500 to 800° C. and the degreasing time is 120 to 300 minutes;

[0025] In the sintering step, the sintering temperature is 1200-1400° C., and the sintering time is 120-240 minutes.

[0026] Compared with the prior art, the method of the present invention has the following beneficial effects:

[0027] The alcohol-based binder disclosed in the present invention uses polyvinyl pyrrolidone as a base material to consolidate metal powders, a surfactant can effectively improve the wetting performance of the binder on the surface of the metal powder, ethylene glycol methyl ether is used as a solvent to greatly reduce the surface tension of the binder, and a stabilizer is added to maintain the chemical uniformity and stability of the binder. The alcohol-based binder disclosed in the present invention has good fluidity and rapid curing performance, and has good compatibility with metal powders, especially titanium alloy metal powders, and is particularly suitable for binder jetting 3D printing of lightweight metal products, especially in the fields of aerospace, biomedicine, etc. It has important application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] none DETAILED DESCRIPTION

[0029] For ease of understanding of the present invention, the present invention will be described more fully below with reference to relevant embodiments. Preferred embodiments of the present invention are provided in the embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0031] One of the purposes of the present invention is to disclose an alcohol-based binder, which comprises, by weight, 10 to 15 parts of polyvinyl pyrrolidone, 5 to 10 parts of a stabilizer, 10 to 20 parts of a surfactant and 55 to 75 parts of a solvent. Among them, the solvent is ethylene glycol monomethyl ether, which has the function of improving the wetting effect and viscosity compared with other solvents, and can better meet the parameter requirements of the print head nozzle jet printing; and ethylene glycol monomethyl ether as a solvent is volatile and has strong permeability, which can appropriately increase the thickness of the printed layer and improve the printing efficiency. The stabilizer can be at least one of 2-pyrrolidone or ethylene acrylic acid; the surfactant can be at least one of diethylene glycol, diethylene glycol and ethylene glycol butyl ether; the molecular weight of polyvinyl pyrrolidone is 40,000 to 60,000 g / mol, the viscosity is suitable and does not affect the degreasing efficiency of the printed product.

[0032] A second object of the present invention is to provide a preparation method, which is applied to the alcohol-based binder described in any of the above embodiments. The preparation method may include the following steps:

[0033] S110, mixing 55 to 75 parts of a solvent and 10 to 20 parts of a surfactant, and stirring for 10 to 20 minutes;

[0034] Add 5 to 10 parts of a stabilizer to the mixture obtained in steps S120 and S110, and stir for 10 to 20 minutes;

[0035] 10 to 15 parts of polyvinyl pyrrolidone are added to the mixture obtained in steps S130 and S120, and the mixture is stirred for 20 to 40 minutes.

[0036] A third object of the present invention is to provide a method of use, which is applied to any of the above-mentioned alcohol-based binders, and the alcohol-based binder can be used for binder jetting 3D printing of metal products.

[0037] Specifically, the production of the metal product may include the following steps:

[0038] S200, 3D printing

[0039] S210, measuring the properties of the metal powder, drying the powder in a vacuum oven and then sieving it, placing the powder in a powder hopper, and installing a working box for a powder spreading device;

[0040] S220, cleaning the print head to ensure that there are no impurities or residues, performing an inkjet test on the print head, and checking the frame loss of the print head;

[0041] S230, import the model to be printed into the printer, set the powder layer thickness to 20 to 80 microns, and determine and set key parameters such as powder feeding speed, powder spreading speed, roller speed, heating lamp temperature, etc. during the printing process;

[0042] S240, the working box descends by one layer thickness, and the powder spreader spreads powder;

[0043] S250, the print head sprays the binder onto the powder layer in a directional manner;

[0044] S260, repeating the above step S240 and the above step S250 until the printing is completed;

[0045] S300, after printing is completed, the work box is placed in a curing device for curing treatment, the curing temperature is 150-200°C, and the curing time is 180-600 minutes;

[0046] S400, placing the working box on a powder cleaning table, removing excess powder, and obtaining a metal green body;

[0047] S500, the metal green body is placed in a degreasing furnace through a ceramic plate for vacuum degreasing treatment, the degreasing temperature is 500-800°C, and the degreasing time is 120-300 minutes;

[0048] S600: The green body after degreasing treatment is placed in a sintering furnace for sintering treatment. The sintering temperature is 1200-1400° C. and the sintering time is 120-240 minutes.

[0049] Embodiment 1

[0050] An alcohol-based binder comprises, by weight, 12 parts of polyvinyl pyrrolidone, 70 parts of ethylene glycol monomethyl ether, 10 parts of diethylene glycol, and 8 parts of 2-pyrrolidone. The average molecular weight of the polyvinyl pyrrolidone is 4000 g / mol.

[0051] The preparation method of the alcohol-based binder of the present invention may include the following steps:

[0052] S110, mixing 10 parts of diethylene glycol and 70 parts of ethylene glycol monomethyl ether, and stirring for 10 minutes;

[0053] 8 parts of 2-pyrrolidone were added to the mixture obtained in steps S120 and S110, and stirred for 10 minutes;

[0054] The mixture obtained in steps S130 and S120 is added with 12 parts of polyvinyl pyrrolidone and stirred for 30 minutes to obtain the alcohol-based binder of this embodiment.

[0055] In this embodiment, the alcohol-based binder is used for binder jetting 3D printing of metal products. The method for making the metal products may include the following steps:

[0056] S200, 3D printing

[0057] S210, measuring the properties of the metal powder, drying the powder in a vacuum oven and then sieving it, placing the powder in a powder hopper, and installing a working box for a powder spreading device;

[0058] It should be noted that, in this embodiment, atomized TC4 powder is used, and the powder particle size is controlled within the range of 0 to 25 μm.

[0059] S220, cleaning the print head to ensure that there are no impurities or residues, performing an inkjet test on the print head, and checking the frame loss of the print head;

[0060] S230, import the model to be printed into the printer, and set the powder layer thickness to 50 microns;

[0061] S240, the working box descends by one layer thickness, and the powder spreader spreads powder;

[0062] S250, the print head sprays the alcohol-based binder of this embodiment onto the powder layer in a directional manner;

[0063] S260, repeating the above step S240 and the above step S250 until the printing is completed;

[0064] S300, after printing is completed, the work box is placed in a curing device for curing, the curing temperature is 150°C, and the curing time is 240 minutes;

[0065] S400, placing the working box on a powder cleaning table, removing excess powder, and obtaining a metal green body;

[0066] S500, the metal green body is placed in a degreasing furnace through a ceramic plate for vacuum degreasing treatment, the degreasing temperature is 550°C, and the degreasing time is 300 minutes;

[0067] S600, the green body after degreasing treatment is placed in a sintering furnace for sintering treatment to obtain a metal product, the sintering temperature is 1300° C., and the sintering time is 180 minutes.

[0068] The metal product prepared in this embodiment has a density of 99.25%, a tensile strength of 570 MPa, and an elongation after fracture of 50%.

[0069] Embodiment 2

[0070] An alcohol-based binder comprises, by weight, 12 parts of polyvinyl pyrrolidone, 70 parts of ethylene glycol monomethyl ether, 5 parts of diethylene glycol, 5 parts of ethylene glycol butyl ether, and 8 parts of 2-pyrrolidone. The average molecular weight of the polyvinyl pyrrolidone is 5000 g / mol.

[0071] The preparation method of the alcohol-based binder of the present invention may include the following steps:

[0072] S110, mixing 5 parts of diethylene glycol, 5 parts of ethylene glycol butyl ether and 70 parts of ethylene glycol monomethyl ether, and stirring for 20 minutes;

[0073] 8 parts of 2-pyrrolidone were added to the mixture obtained in steps S120 and S110, and stirred for 20 minutes;

[0074] The mixture obtained in steps S130 and S120 is added with 12 parts of polyvinyl pyrrolidone and stirred for 30 minutes to obtain the alcohol-based binder of this embodiment.

[0075] In this embodiment, the alcohol-based binder is used for binder jetting 3D printing of metal products. The method for making the metal products may include the following steps:

[0076] S200, 3D printing

[0077] S210, measuring the properties of the metal powder, drying the powder in a vacuum oven and then sieving it, placing the powder in a powder hopper, and installing a working box for a powder spreading device;

[0078] It should be noted that, in this embodiment, aerosolized 316L powder is used, and the powder particle size is controlled within the range of 0 to 25 μm.

[0079] S220, cleaning the print head to ensure that there are no impurities or residues, performing an inkjet test on the print head, and checking the frame loss of the print head;

[0080] S230, import the model to be printed into the printer, and set the powder layer thickness to 50 microns;

[0081] S240, the working box descends by one layer thickness, and the powder spreader spreads powder;

[0082] S250, the print head sprays the alcohol-based binder of this embodiment onto the powder layer in a directional manner;

[0083] S260, repeating the above step S240 and the above step S250 until the printing is completed;

[0084] S300, after printing is completed, the work box is placed in a curing device for curing, the curing temperature is 200°C, and the curing time is 180 minutes;

[0085] S400, placing the working box on a powder cleaning table, removing excess powder, and obtaining a metal green body;

[0086] S500, the metal green body is placed in a degreasing furnace through a ceramic plate for vacuum degreasing treatment, the degreasing temperature is 800°C, and the degreasing time is 120 minutes;

[0087] S600. The green body after degreasing treatment is placed in a sintering furnace for sintering treatment to obtain a metal product. The sintering temperature is 1385° C. and the sintering time is 180 minutes.

[0088] The metal product prepared in this embodiment has a density of 98.94%, a tensile strength of 565 MPa, and an elongation after fracture of 48%.

[0089] Embodiment 3

[0090] An alcohol-based binder comprises, by weight, 10 parts of polyvinyl pyrrolidone, 70 parts of ethylene glycol monomethyl ether, 5 parts of diethylene glycol, 5 parts of ethylene glycol butyl ether, and 10 parts of 2-pyrrolidone. The average molecular weight of the polyvinyl pyrrolidone is 6000 g / mol.

[0091] The preparation method of the alcohol-based binder of the present invention may include the following steps:

[0092] S110, mixing 5 parts of diethylene glycol, 5 parts of ethylene glycol butyl ether and 70 parts of ethylene glycol monomethyl ether, and stirring for 20 minutes;

[0093] 10 parts of 2-pyrrolidone were added to the mixture obtained in steps S120 and S110, and stirred for 20 minutes;

[0094] The mixture obtained in steps S130 and S120 is added with 10 parts of polyvinyl pyrrolidone and stirred for 30 minutes to obtain the alcohol-based binder of this embodiment.

[0095] In this embodiment, the alcohol-based binder is used for binder jetting 3D printing of metal products. The method for making the metal products may include the following steps:

[0096] S200, 3D printing

[0097] S210, measuring the properties of the metal powder, drying the powder in a vacuum oven and then sieving it, placing the powder in a powder hopper, and installing a working box for a powder spreading device;

[0098] It should be noted that, in this embodiment, aerosolized 316L powder is used, and the powder particle size is controlled within the range of 0 to 25 μm.

[0099] S220, cleaning the print head to ensure that there are no impurities or residues, performing an inkjet test on the print head, and checking the frame loss of the print head;

[0100] S230, import the model to be printed into the printer, and set the powder layer thickness to 50 microns;

[0101] S240, the working box descends by one layer thickness, and the powder spreader spreads powder;

[0102] S250, the print head sprays the alcohol-based binder of this embodiment onto the powder layer in a directional manner;

[0103] S260, repeating the above step S240 and the above step S250 until the printing is completed;

[0104] S300, after printing is completed, the work box is placed in a curing device for curing, the curing temperature is 200°C, and the curing time is 180 minutes;

[0105] S400, placing the working box on a powder cleaning table, removing excess powder, and obtaining a metal green body;

[0106] S500, the metal green body is placed in a degreasing furnace through a ceramic plate for vacuum degreasing treatment, the degreasing temperature is 800°C, and the degreasing time is 120 minutes;

[0107] S600. The green body after degreasing treatment is placed in a sintering furnace for sintering treatment to obtain a metal product. The sintering temperature is 1385° C. and the sintering time is 180 minutes.

[0108] The metal product prepared in this embodiment has a density of 98.70%, a tensile strength of 501 MPa, and an elongation after fracture of 42%.

[0109] Embodiment 4

[0110] An alcohol-based binder comprises, by weight, 8 parts of polyvinyl pyrrolidone, 70 parts of ethylene glycol monomethyl ether, 10 parts of diethylene glycol, and 12 parts of ethylene acrylic acid. The average molecular weight of the polyvinyl pyrrolidone is 4000 g / mol.

[0111] The preparation method of the alcohol-based binder of the present invention may include the following steps:

[0112] S110, mixing 10 parts of diethylene glycol and 70 parts of ethylene glycol monomethyl ether, and stirring for 20 minutes;

[0113] 12 parts of ethylene acrylic acid are added to the mixture obtained in steps S120 and S110, and stirred for 20 minutes;

[0114] 8 parts of polyvinyl pyrrolidone are added to the mixture obtained in steps S130 and S120, and the mixture is stirred for 40 minutes to obtain the alcohol-based binder of this embodiment.

[0115] In this embodiment, the alcohol-based binder is used for binder jetting 3D printing of metal products. The method for making the metal products may include the following steps:

[0116] S200, 3D printing

[0117] S210, measuring the properties of the metal powder, drying the powder in a vacuum oven and then sieving it, placing the powder in a powder hopper, and installing a working box for a powder spreading device;

[0118] It should be noted that, in this embodiment, aerosolized 316L powder is used, and the powder particle size is controlled within the range of 0 to 25 μm.

[0119] S220, cleaning the print head to ensure that there are no impurities or residues, performing an inkjet test on the print head, and checking the frame loss of the print head;

[0120] S230, import the model to be printed into the printer, and set the powder layer thickness to 50 microns;

[0121] S240, the working box descends by one layer thickness, and the powder spreader spreads powder;

[0122] S250, the print head sprays the alcohol-based binder of this embodiment onto the powder layer in a directional manner;

[0123] S260, repeating the above step S240 and the above step S250 until the printing is completed;

[0124] S300, after printing is completed, the work box is placed in a curing device for curing, the curing temperature is 150°C, and the curing time is 240 minutes;

[0125] S400, placing the working box on a powder cleaning table, removing excess powder, and obtaining a metal green body;

[0126] S500, the metal green body is placed in a degreasing furnace through a ceramic plate for vacuum degreasing treatment, the degreasing temperature is 550°C, and the degreasing time is 300 minutes;

[0127] S600, the green body after degreasing treatment is placed in a sintering furnace for sintering treatment to obtain a metal product, the sintering temperature is 1300° C., and the sintering time is 180 minutes.

[0128] The metal product prepared in this embodiment has a density of 99.85%, a tensile strength of 585 MPa, and an elongation after fracture of 55%.

[0129] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. An alcohol-based binder, characterized in that: The invention comprises, by weight: 10 to 15 parts of polyvinyl pyrrolidone, 5 to 10 parts of a stabilizer, 10 to 20 parts of a surfactant and 55 to 75 parts of a solvent.

2. The alcohol-based binder according to claim 1, characterized in that The solvent is ethylene glycol monomethyl ether.

3. The alcohol-based binder according to claim 1, characterized in that The stabilizer is at least one of 2-pyrrolidone or ethylene acrylic acid.

4. The alcohol-based binder according to claim 1, characterized in that The surfactant is at least one of diethylene glycol, diethylene glycol and ethylene glycol butyl ether.

5. The alcohol-based binder according to claim 1, characterized in that The molecular weight of the polyvinyl pyrrolidone is 40000-60000 g / mol.

6. A preparation method, applied to the alcohol-based binder according to any one of claims 1 to 5, characterized in that: The steps include: S110, mixing the solvent and the surfactant, and stirring for 10 to 20 minutes; S120, adding the stabilizer and stirring for 10 to 20 minutes; S130, adding the polyvinyl pyrrolidone and stirring for 20 to 40 minutes.

7. A method of use, applied to the alcohol-based binder according to any one of claims 1 to 5, characterized in that: The alcohol-based binder is used for binder jetting 3D printing of metal powders.

8. The method of use according to claim 7, characterized in that: The steps include: S210, importing the printing model into the 3D printer; S220, the working box descends a layer thickness, and the powder spreader spreads powder; the layer thickness is set to 20 to 80 microns; S230, the print head sprays the alcohol-based binder onto the powder layer in a directional manner; S240, repeating the step S220 and the step S230 until printing is completed.

9. The method of use according to claim 8, characterized in that: After the step S240, the printed product is further cured, degreased and sintered in sequence; In the curing step, the curing temperature is 150 to 200° C. and the curing time is 180 to 600 minutes; In the degreasing step, the degreasing temperature is 500 to 800° C. and the degreasing time is 120 to 300 minutes; In the sintering step, the sintering temperature is 1200-1400° C., and the sintering time is 120-240 minutes.