Manufacturing mold and preparation method of riser tube for high-temperature alloy

By adopting coating + grouting forming method and mold design in high-temperature alloy anti-gravity casting, the chemical stability and fitting problems of the lifting pipe are solved, and low-cost, high-precision and high-stability ceramic lifting pipes are achieved. , suitable for anti-gravity casting of high-temperature alloys, improving process efficiency and product performance.

CN119036619APending Publication Date: 2024-11-29NORTHWESTERN POLYTECHNICAL UNIV +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410953414.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In high-temperature alloy anti-gravity casting, existing liquid lifting pipes have problems such as low chemical stability, limiting plates cannot fully fit with the pipe body, complex process and high cost, making it difficult to meet the needs of high dimensional accuracy and low cost.

Method used

A mold including inner cavity wax mold, cover plate and half mold is prepared by coating and hanging + grouting forming method. The mold is tightly clamped through positioning columns and groove structures, combining the tapered cavity design and multi-layer slurry Apply to ensure high precision and chemical stability of the lift tube.

Benefits of technology

It realizes low-cost, high dimensional accuracy and high chemical stability of the ceramic liquid lift tube, improves the overall strength and sealing of the liquid lift tube, is suitable for high-temperature alloy anti-gravity casting, and has a process cycle that is better than traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119036619A_ABST
    Figure CN119036619A_ABST
Patent Text Reader

Abstract

The invention relates to a manufacturing mold and a preparation method of a riser tube for a high-temperature alloy. The manufacturing mold is characterized by comprising an inner cavity wax mold, a first half mold, a second half mold and a cover plate, the second half mold and the first half mold are symmetrical in structure, when the two half molds are closed, the positioning pin is inserted into the positioning hole, the cover plate is fixed to the top face of the closed mold, a riser tube main body cavity is formed in the center of the closed mold, a tube body at the bottom of the riser tube main body cavity is of a conical structure, and attachment and sealing of the riser tube and a casting shell are achieved. The preparation method comprises the following steps: preparing the riser tube inner cavity wax mold, coating the inner cavity wax mold, fixing the mold, grouting, demolding and roasting. A mold grouting method is adopted, and the characteristics of uniform coating, high binding force and the like of a coating and hanging method are integrated on the basis of a conventional grouting method, so that the flange part of the riser tube and the tube body are integrally formed. The prepared riser tube is high in size precision, resistant to high temperature and low in cost, and the overall strength and chemical stability of the riser tube are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of a riser tube for counter-gravity casting of a high-temperature alloy, and in particular to a manufacturing mold and a preparation method of a riser tube for a high-temperature alloy. Background Art

[0002] With the rapid development of major equipment in the fields of aerospace, etc., the current hot end components are developing in the direction of lightweight, integration, and thin-walled, and the molding quality requirements of castings are getting higher and higher. Traditional gravity casting cannot meet structural requirements due to a series of casting defects such as undercasting, uneven structure, shrinkage and shrinkage holes. Therefore, the anti-gravity casting process widely used in aluminum and magnesium alloy systems has received more attention. Anti-gravity casting is a casting process that can achieve continuous filling of molten metal from bottom to top and solidification from top to bottom under the action of external pressure. It has the characteristics of stable filling, reduced turbulence and inclusions of molten metal, and timely shrinkage compensation. However, due to the constraints of key issues such as pressure parameter setting in the casting process, material selection and structural design of the riser, and high-temperature sealing of the riser and equipment, the current anti-gravity casting technology of high-temperature alloys is still in the basic research stage.

[0003] High-temperature alloys have the characteristics of high melting point, high density and high viscosity. The preparation process of the riser tube must take into account air tightness, chemical stability, strength and thermal shock resistance. At present, the anti-gravity casting riser tubes for high-temperature alloys mainly include corundum-mullite-based riser tubes, silica-based riser tubes, composite riser tubes, etc. Among them, the corundum-mullite-based riser tubes themselves have certain microcracks and holes, and the thermal shock resistance cannot meet the high air tightness requirements; the silica-based riser tube has a low thermal expansion coefficient, but it is very easy to react with active elements in the molten metal, and the chemical stability is poor; the metal tube body in the composite riser tube is usually not completely fitted with non-metallic materials, and the preparation method is complex and costly.

[0004] Chinese patent CN 219254098 U discloses a riser pipe prepared by connecting multiple non-metallic refractory layers with refractory fiber media. One end of the pipe body has a detachable limit plate. The good combination of non-metallic materials in the pipe body improves the thermal shock resistance of the riser pipe. However, the limit plate in the split riser pipe cannot be completely fitted with the pipe body. When the ceramic material of the pipe body expands and contracts due to temperature changes, the limit plate cannot change synchronously. The overall sealing of the riser pipe limits the subsequent metal liquid filling process.

[0005] Therefore, a low-cost integrated riser tube for high-temperature alloys with high dimensional accuracy and high chemical stability is urgently needed to provide a technical basis for the development and application of anti-gravity casting technology for high-temperature alloys. Summary of the invention

[0006] The purpose of the present invention is to provide a mold for preparing a riser tube for a high-temperature alloy in order to address the problems of low chemical stability and inability of the limit plate to fully fit the tube body in the prior art. An integrated ceramic riser tube with low cost, high dimensional accuracy and chemical stability is prepared by a coating + grouting forming method.

[0007] To achieve the above object, the technical solution adopted by the present invention is: a mold for manufacturing a riser tube for high temperature alloy, comprising an inner cavity wax mold, a cover plate, a first half mold and a second half mold corresponding to and matching the first half mold;

[0008] The inner wax mold structure is cylindrical and matches the inner diameter of the riser tube. The upper and lower ends of the inner wax mold are respectively provided with an upper positioning column and a lower positioning column for fixing and positioning the inner wax mold. The cross section of the lower positioning column is a combination of a semicircle and a semi-square.

[0009] A symmetrically distributed first threaded hole is provided at the top of the first half mold, a first half cavity is provided at the axial middle of the first half mold, diagonally distributed positioning pins are provided on the axial planes on both sides of the cavity, a semi-square groove for fixing and positioning the lower positioning column is provided at the bottom of the first half mold, that is, below the first half cavity, and first handles are provided on both sides of the first half mold;

[0010] The top of the second half mold is provided with second threaded holes which are symmetrically distributed, and the axial middle part of the second half mold is provided with a second half cavity corresponding to the first half cavity; axial planes on both sides of the second cavity are provided with positioning holes which are matched with the positioning pins, and at the bottom of the second half mold, that is, below the second cavity, a semicircular groove corresponding to the semi-square groove is provided, and the semi-square groove and the semicircular groove are combined to form a fixing hole for fixing and positioning the lower positioning column, and second handles are provided on both sides of the second half mold;

[0011] A limiting hole matching the upper positioning column is provided at the center of the cover plate for limiting the mold shell of the liquid riser, and feed ports distributed in a cross-shaped ring are provided around the limiting hole, and circular grooves matching and corresponding to the first threaded hole and the second threaded hole are provided around the cover plate;

[0012] The first half mold is combined with the second half mold, the positioning pin is inserted into the positioning hole, the cover plate is arranged on the top surface of the combined mold, and the bolts are screwed into the circular groove to fix the cover plate and the combined mold to form a riser tube mold. The center of the combined mold is formed by the first half cavity and the second half cavity to form the riser tube main body cavity.

[0013] Furthermore, the tube body at the bottom of the main cavity of the riser tube is a conical structure with a conical angle of 58°-62° and a conical height of 7-9mm, which is used to achieve the fitting and sealing of the riser tube and the casting shell; 15 to 20mm of the tube body is reserved at the upper end of the riser tube flange on the upper part of the riser tube body to prevent the molten metal from escaping.

[0014] The present invention also provides a method for preparing a riser tube for a high-temperature alloy, the steps of which are as follows:

[0015] Step 1: using a laser rapid prototyping machine to prepare a riser tube inner cavity resin mold, and then performing wax immersion treatment on the riser tube inner cavity resin mold to increase surface finish and strength, thereby obtaining a riser tube inner cavity wax mold;

[0016] Step 2: Preliminary coating is performed on the inner wax mold of the riser tube, which includes coating at least two layers of slurry on the surface of the inner wax mold of the riser tube to form an inner shell, coating at least two layers of slurry on the surface of the inner shell to form a transition shell, and coating 4 to 5 layers of slurry on the surface of the transition shell to form an outer shell, leaving a 6 to 8 mm grouting space to ensure that the riser tube has a certain strength, air tightness and smoothness;

[0017] Step 3: accurately place the coated inner wax mold in the riser tube mold, fix the inner wax mold in the fixing hole through the lower positioning column, close the first and second molds with the help of the first and second handles, insert the positioning pins into the positioning holes, fix the cover plate to the top of the riser tube mold, pass the inner wax mold through the limiting holes through the upper positioning column, and then screw the bolts into the circular grooves to tighten the riser tube mold, further reducing the mold gap;

[0018] Step 4: Use a handheld mixer to control the speed of the grouting material to 350-400r / min, stir it evenly for 5-10 minutes, and then inject it into the riser tube mold through the feed port, and the grouting time is controlled within 5 minutes; after the grouting is completed and vibrated and compacted, the riser tube mold with the grouting material is placed in a booster tank for boosting treatment, and the boosting pressure is 350-450kPa to ensure that there are no pores inside the cavity;

[0019] Step 5: After the riser tube mold is naturally dried for 68-74 hours, demoulding is performed to obtain a riser tube mold shell;

[0020] Step 6: Place the riser tube mold shell in a resistance furnace at 750°C for dewaxing treatment and keep it warm for 1 hour. After the wax mold of the inner cavity of the riser tube is completely removed, heat it to 950°C and pre-sinter it for 2 hours. Then sinter it at 1150°C for 4 hours to ceramicize it and cool it with the furnace. Then grind its surface to ensure that the upper and lower surfaces of the riser tube flange are flat to obtain the riser tube.

[0021] Furthermore, the slurry in step 2 includes an inner layer slurry, a transition layer slurry and an outer layer slurry, and the specific process of the initial coating is:

[0022] The inner wax mold (1) is completely immersed in the inner layer slurry for 5 to 10 seconds, and then the inner layer refractory sand is evenly sprinkled on the surface thereof, and the inner wax mold (1) is placed in a ventilated environment with a humidity of 50 to 70% and a temperature of 15 to 28° C., and is naturally air-dried to obtain an inner layer shell;

[0023] The inner shell is immersed in the transition layer slurry for 15 to 30 seconds, then the transition layer refractory sand is evenly sprinkled on the surface, and it is placed in a ventilated environment with a humidity of 50 to 70% and a temperature of 15 to 28°C, and the transition layer shell is obtained after natural air drying;

[0024] The transition layer shell is immersed in the outer layer slurry for 15 to 30 seconds, then the outer layer refractory sand is evenly sprinkled on its surface, and it is placed in a ventilated environment with a humidity of 50 to 70% and a temperature of 15 to 28° C., and the outer shell is obtained after natural air drying.

[0025] Furthermore, the grouting material in step 4 is mixed by an inner layer slurry, an outer layer slurry, zircon sand, fine upper sand, coarse upper sand and refractory fiber. The mixing process is: the inner layer slurry and the outer layer slurry are mixed and stirred at a low speed for 5 to 8 minutes, and then zircon sand, fine upper sand, coarse upper sand and refractory fiber are added in sequence to form a slurry. When the mixed slurry falls freely, it is in the form of discontinuous flocs, which meets the use requirements.

[0026] Furthermore, the inner layer slurry includes silica sol, 325 mesh zircon powder, defoamer and wetting agent, wherein: the mass ratio of silica sol to 325 mesh zircon powder is 1:3-4; the defoamer model is FA905, and the dosage accounts for 0.05% of the total mass; the wetting agent model is WET-10S, and the dosage accounts for 0.1% of the total mass.

[0027] Furthermore, the transition layer slurry includes silica sol, 200-mesh powder and defoamer, wherein the mass ratio of silica sol to 200-mesh powder is 1:3-4, and the defoamer model is FA905, and the amount is 0.05% of the total mass.

[0028] The outer layer slurry is the same as the transition layer slurry.

[0029] Furthermore, the inner layer of refractory sand is 80-120 mesh zircon sand; the transition layer of refractory sand is 30-60 mesh upper sand; and the outer layer of refractory sand is 16-30 mesh upper sand.

[0030] Furthermore, the calcination treatment in step 6 is specifically as follows: the riser tube mold shell is placed in a resistance furnace at 750°C for dewaxing treatment and kept warm for 1 hour, and after the wax mold of the inner cavity of the riser tube is completely removed, the temperature is raised to 950°C for pre-sintering for 2 hours, and then sintered at 1150°C for 4 hours to ceramicize it and cool it with the furnace.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. The bottom of the mold designed by the present invention is provided with a square and circular positioning groove, which is used to fix the inner cavity wax mold and limit its freedom in the mold. After the first half mold and the second half mold are combined, the top is fixed with a cover plate. The upper positioning column of the inner cavity wax mold passes through the limiting hole in the middle of the cover plate to lock the two half molds, further narrowing the mold gap and laying a technological foundation for subsequent complete grouting forming.

[0033] 2. The bottom tube of the main cavity of the riser tube of the present invention is designed as a conical structure, which is used to achieve the fit between the riser tube and the casting shell, and has a good sealing effect while having a certain drainage effect on the molten metal.

[0034] 3. The present invention adopts the mold grouting method, which integrates the characteristics of the coating method such as uniform coating and strong bonding force on the basis of the conventional grouting method, so that the flange part of the riser pipe and the pipe body can be integrally formed.

[0035] 4. The prepared riser tube has the characteristics of high dimensional accuracy, high temperature resistance and low cost, which improves the overall strength and chemical stability of the riser tube, and the single process cycle is better than the conventional riser tube preparation method. It can also be used in the anti-gravity casting process of metal materials such as aluminum alloy and cast steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Schematic diagram of the inner cavity wax mold structure of the mold of the present invention;

[0037] Figure 2 It is a schematic diagram of the first half mold structure of the mold of the present invention;

[0038] Figure 3 It is a schematic diagram of the second half mold structure of the mold of the present invention;

[0039] Figure 4 It is a schematic diagram of the cover plate structure of the mold of the present invention;

[0040] Figure 5 It is a schematic diagram of the two half molds of the present invention being molded together;

[0041] Figure 6 It is a cross-sectional view of two half molds of the present invention;

[0042] Figure 7 A schematic diagram of the structure of the liquid riser prepared in the present invention;

[0043] In the figure: 1-inner cavity wax mold, 12-upper positioning column, 13-lower positioning column, 2-first half mold, 21-first threaded hole, 22-positioning pin, 23-semi-square groove, 24-first handle; 3-second half mold, 31-second threaded hole, 32-positioning hole, 33-semicircular groove, 34-second handle; 4-cover plate, 41-limiting hole, 42-feed port, 43-circular groove; 5-liquid lifting pipe, 51-liquid lifting pipe flange. DETAILED DESCRIPTION

[0044] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0045] In order to achieve the above object, the present invention provides the following specific implementation methods:

[0046] Example 1: Figure 1-7 As shown, a mold for manufacturing a riser tube for high temperature alloys comprises an inner cavity wax mold 1, a cover plate 4, a first half mold 2 and a second half mold 3 corresponding to and matching the first half mold 2;

[0047] like Figure 1 As shown, the inner cavity wax mold 1 is made of polystyrene resin powder by laser rapid prototyping technology. The structure of the inner cavity wax mold 1 is cylindrical and matches the inner diameter of the riser 5. The inner cavity wax mold 1 has a diameter of 40 mm and a height of 400 mm. The upper and lower ends of the inner cavity wax mold 1 are respectively provided with an upper positioning column 11 and a lower positioning column 12 for fixing and positioning the inner cavity wax mold 1. The cross section of the lower positioning column 12 is a combination of a semicircle and a semi-square.

[0048] In order to improve the dimensional accuracy and surface finish of the inner wax mold 1, the polystyrene resin wax mold is treated with wax dipping: first, the polystyrene resin wax mold is slowly immersed in a wax dipping machine, in which low-temperature white wax liquid with a temperature of 50 to 70°C is melted; then, the mold is placed in the low-temperature white wax for 2 to 3 seconds, taken out, and subjected to finishing treatment after standing at room temperature; then, the surface of the wax mold is polished with 600-mesh water sandpaper; finally, soapy water is used for degreasing treatment, the wax mold is rinsed with clean water, and placed in a dry and ventilated place at room temperature to dry naturally.

[0049] like Figure 2 As shown, a symmetrically distributed first threaded hole 21 is provided on the top of the first half mold 2, a first half cavity is provided in the axial middle of the first half mold 2, and diagonally distributed positioning pins 22 are provided on the axial planes on both sides of the cavity, and a semi-square groove 23 for fixing and positioning the lower positioning column 12 is provided at the bottom of the first half mold 2, that is, below the first half cavity, and a first handle 24 is provided on both sides of the first half mold 2;

[0050] like Figure 3 As shown, the top of the second half mold 3 is provided with symmetrically distributed second threaded holes 31, and the axial middle part of the second half mold 3 is provided with a second half cavity corresponding to the first half cavity; axial planes on both sides of the second cavity are provided with positioning holes 32 matched with the positioning pin 22, and a semicircular groove 33 corresponding to the semi-square groove 23 is provided at the bottom of the second half mold 3, that is, below the second cavity, and the semi-square groove 23 and the semicircular groove 33 are combined to form a fixing hole for fixing and positioning the lower positioning column 12, and second handles 34 are provided on both sides of the second half mold 3;

[0051] like Figure 4 As shown, a limiting hole 41 matching the upper positioning column 11 is provided at the center of the cover plate 4, which is used for limiting the shell of the riser 5. The limiting hole 41 and the upper positioning column 11 of the inner cavity wax mold 1 have a diameter of 20 mm. Feed ports 42 distributed in a cross-shaped ring are provided around the limiting hole 41. The width of the feed port 42 is 30 mm. Circular grooves 43 matching and corresponding to the first threaded hole 21 and the second threaded hole 31 are provided around the cover plate 4.

[0052] like Figure 5 , Figure 6 As shown, when the first half mold 2 and the second half mold 3 are closed, the positioning pin 22 is inserted into the positioning hole 32, the cover plate 4 is arranged on the top surface of the closed mold, and the bolts are screwed into the circular groove 43 to fix the cover plate 4 and the combined mold to form a riser tube mold. The center of the closed mold is formed by the combination of the first half cavity and the second half cavity to form a riser tube main cavity. The diameter of the tube body in the riser tube main cavity is 70 mm, the total height of the tube body is 400 mm, and the diameter of the riser tube flange is 100 mm.

[0053] like Figure 7 As shown, the bottom tube of the main cavity of the riser tube is a conical structure, the conical angle at the tube mouth is 60°, and the conical height is 8mm, so as to avoid stress concentration at the contact end with the casting shell and affect the overall air tightness of the equipment, and at the same time play a certain role in draining the molten metal. The upper end of the riser tube flange 51 on the upper part of the riser tube 5 is reserved with a tube body of 15 to 20 mm to prevent the molten metal from escaping.

[0054] Embodiment 2: A method for manufacturing a liquid riser tube for high temperature alloys, the specific steps are as follows:

[0055] Step 1: Prepare a wax model 1 of the inner cavity of the riser tube. According to the inner diameter of the riser tube being 45 mm and the total height of the tube being 400 mm, input the inner cavity three-dimensional model and processing parameters into a laser rapid prototyping machine; add polystyrene resin powder for printing into the laser rapid prototyping machine, and obtain the wax model 1 of the inner cavity of the riser tube by laser rapid prototyping;

[0056] Step 2: Coating the inner wax model. The printed inner wax model 1 is preliminarily coated, that is, the inner shell is formed by coating at least two layers of slurry on the surface of the inner wax model 1, the transition shell is formed by coating at least two layers of slurry on the surface of the inner shell, and the outer shell is formed by coating 4 to 5 layers of slurry on the surface of the transition shell, leaving 6 to 8 mm of grouting space to ensure that the riser has a certain strength, airtightness and smoothness.

[0057] The specific process of preliminary painting is:

[0058] Preparation of inner slurry: silica sol and 325 mesh zircon powder are prepared in a mass ratio of 1:3, and the mixer is stirred at a low speed of 350r / min for about 5 minutes, and then 0.05wt.% of FA905 defoamer and 0.1wt.% of WET-10S wetting agent are added and stirred at high speed for about 7-8 minutes. The inner wax mold is completely immersed in the inner slurry for 5-10 seconds, and then 80-120 mesh zircon sand is spread on its surface, and placed in a ventilated environment with a humidity of 50-70% and a temperature of 15-28℃. After natural air drying, the inner shell of the riser tube is obtained. Zircon powder / zircon sand has good high temperature resistance, chemical stability and corrosion resistance, which ensures that the molten metal fills the mold smoothly without reacting with the riser tube.

[0059] Prepare transition layer slurry: silica sol and 200 mesh Shangdian powder are prepared in a mass ratio of 1:3, and 0.05wt.% FA905 defoamer is added. The inner shell of the riser tube is immersed in the transition layer slurry for 15-30s, and then 30-60 mesh Shangdian sand is spread on its surface, and it is placed in a ventilated environment with a humidity of 50-70% and a temperature of 15-28°C. After natural air drying, the transition layer shell of the riser tube is obtained. Shangdian powder / Shangdian sand has good high temperature resistance and a linear expansion coefficient similar to that of the inner layer material, which prevents the pipe body from unevenly expanding and cracking due to heating.

[0060] The outer layer slurry is prepared in the same way as the transition layer slurry. The riser transition layer shell is immersed in the outer layer slurry for 15 to 30 seconds, and then 16 to 30 mesh sand is spread on its surface, and it is placed in a ventilated environment with a humidity of 50 to 70% and a temperature of 15 to 28°C. After natural air drying, the initially coated riser shell is obtained.

[0061] Step 3: The coated inner wax mold 1 is accurately placed in the riser tube mold. The inner wax mold 1 is fixed in the fixing hole by the lower positioning column 12. The first half mold 2 and the second half mold 3 are closed by means of the first handle 24 and the second handle 34. The positioning pin 22 is inserted into the positioning hole 32 to fix the cover plate 4 to the top of the riser tube mold. The inner wax mold 1 passes through the limiting hole 41 through the upper positioning column 11, and then the bolt is screwed into the circular groove 43 to tighten the riser tube mold, thereby further reducing the mold gap.

[0062] Step 4: Grouting. The grouting material is evenly stirred for 5 to 10 minutes using a hand-held mixer at a speed of 400 r / min, and then injected into the mold. The grouting time is controlled within 5 minutes. After the grouting is completed, the mold is pressurized to ensure that there are no pores inside the cavity. The pressurization pressure is 400 kPa. The grouting material is mixed with inner layer slurry, outer layer slurry, zircon sand, fine upper sand, coarse upper sand, and refractory fiber.

[0063] Step 5: Demolding. After the mold is naturally dried for 72 hours, demoulding is performed.

[0064] Step 6: Firing treatment. The demoulded riser shell is placed in a resistance furnace at 750°C for dewaxing treatment and kept warm for 1 hour. After the inner wax mold is completely removed, the temperature is raised to 950°C for pre-sintering for 2 hours, and then sintered at 1150°C for 4 hours to ceramicize it and cool it with the furnace; the surface of the prepared ceramic riser is polished to ensure that the upper and lower surfaces of the riser flange are flat, and later with the sealing ring and refractory cotton to achieve the overall sealing of the anti-gravity casting equipment and the casting shell.

[0065] Embodiment 3: A method for manufacturing a liquid riser tube for high temperature alloys, the specific steps are as follows:

[0066] Step 1: Prepare a wax model of the inner cavity of the riser tube, the same as in Example 2.

[0067] Step 2: coating the inner wax mold, and the coating layers are uniformly coated from the inside to the outside according to the ratio of inner layer: transition layer: outer layer = 1:1:2. The specific process is the same as Example 2, except that the inner layer slurry silica sol and 325 mesh zircon powder are prepared in a mass ratio of 1:4, and the transition layer slurry silica sol and 200 mesh upper powder are prepared in a mass ratio of 1:4.

[0068] Step 3: Fix the mold, same as in Example 2.

[0069] Step 4: Grouting, same as Example 2.

[0070] Step 5: demoulding, same as Example 2.

[0071] Step 6: calcination treatment, same as in Example 2.

[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A mold for making a riser tube for high temperature alloys, characterized in that: It comprises an inner cavity wax mold (1), a cover plate (4), a first half mold (2), and a second half mold (3) corresponding to and matching the first half mold (2); The inner cavity wax mold (1) is cylindrical in shape and matches the inner diameter of the riser tube (5). An upper positioning column (11) and a lower positioning column (12) for fixing and positioning the inner cavity wax mold (1) are respectively arranged at the upper and lower ends of the axial direction of the inner cavity wax mold (1); The top of the first half mold (2) is provided with symmetrically distributed first threaded holes (21); the axial middle part of the first half mold (2) is provided with a first half cavity; axial planes on both sides of the cavity are provided with diagonally distributed positioning pins (22); the bottom of the first half mold (2), that is, below the first half cavity, is provided with a semi-square groove (23) for fixing and positioning the lower positioning column (12); and first handles (24) are provided on both sides of the first half mold (2); The top of the second half mold (3) is provided with symmetrically distributed second threaded holes (31); the axial middle part of the second half mold (3) is provided with a second half cavity corresponding to the first half cavity; axial planes on both sides of the second cavity are provided with positioning holes (32) matched with the positioning pin (22); the bottom of the second half mold (3), that is, below the second cavity, is provided with a semicircular groove (33) corresponding to the semi-square groove (23); the semi-square groove (23) and the semicircular groove (33) are combined to form a fixing hole for fixing and positioning the lower positioning column (12); and second handles (34) are provided on both sides of the second half mold (3); The center of the cover plate (4) is provided with a limiting hole (41) matching with the upper positioning column (11) and used for limiting the mold shell of the liquid riser (5); the limiting hole (41) is surrounded by feeding ports (42) distributed in a cross-shaped ring shape; the cover plate (4) is surrounded by circular grooves (43) matching and corresponding to the first threaded hole (21) and the second threaded hole (31); The first half mold (2) and the second half mold (3) are molded together, the positioning pin (22) is inserted into the positioning hole (32), the cover plate (4) is arranged on the top surface of the mold, and the bolts are screwed into the circular groove (43) to fix the cover plate (4) and the combined mold to form a riser tube mold. The center of the mold is formed by the combination of the first half cavity and the second half cavity to form a riser tube main body cavity.

2. A mold for making a riser tube for a high temperature alloy as claimed in claim 1, characterized in that The bottom tube body of the main cavity of the riser tube is a conical structure with a conical angle of 58°-62° and a conical height of 7-9 mm, which is used to achieve the fit and sealing between the riser tube (5) and the casting shell; the upper end of the riser tube flange (51) on the upper part of the tube body of the riser tube (5) reserves 15 to 20 mm of the tube body to prevent the metal liquid from escaping.

3. A method for preparing a liquid riser tube for high temperature alloys, characterized in that Here are the steps: Step 1: using a laser rapid prototyping machine to prepare a riser tube inner cavity resin mold, and then performing wax immersion treatment on the riser tube inner cavity resin mold to increase surface finish and strength, thereby obtaining a riser tube inner cavity wax mold (1); Step 2: Preliminary coating is performed on the inner wax mold (1) of the riser tube, the preliminary coating includes coating at least two layers of slurry on the surface of the inner wax mold (1) of the riser tube to form an inner shell, coating at least two layers of slurry on the surface of the inner shell to form a transition shell, and coating 4 to 5 layers of slurry on the surface of the transition shell to form an outer shell, leaving a 6 to 8 mm grouting space to ensure that the riser tube has a certain strength, air tightness and smoothness; Step 3: The coated inner wax mold (1) is accurately placed in the riser tube mold. The inner wax mold (1) is fixed in the fixing hole by the lower positioning column (12). The first half mold (2) and the second half mold (3) are closed by means of the first handle (24) and the second handle (34). The positioning pin (22) is inserted into the positioning hole (32). The cover plate (4) is fixed to the top of the riser tube mold. The inner wax mold (1) passes through the limiting hole (41) through the upper positioning column (11). Then, the bolt is screwed into the circular groove (43) to tighten the riser tube mold, thereby further reducing the mold gap. Step 4: using a handheld mixer, controlling the speed to 350-400 r / min, uniformly stirring the grouting material for 5-10 minutes, and then injecting it into the riser tube mold through the feed port (42), and the grouting time is controlled within 5 minutes; after the grouting is completed and vibrated and compacted, the riser tube mold with the grouting material is placed in a booster tank for boosting treatment, and the boosting pressure is 350-450 kPa to ensure that there are no pores inside the cavity; Step 5: After the riser tube mold is naturally dried for 68-74 hours, demoulding is performed to obtain a riser tube mold shell; Step 6: After the riser tube mold shell is calcined, its surface is polished to ensure that the upper and lower surfaces of the riser tube flange (51) are flat, thereby obtaining the riser tube.

4. The method for preparing a riser tube for a high temperature alloy according to claim 3, characterized in that: The slurry in step 2 includes inner layer slurry, transition layer slurry and outer layer slurry, and the specific process of preliminary coating is: The inner wax mold (1) is completely immersed in the inner layer slurry for 5 to 10 seconds, and then the inner layer refractory sand is evenly sprinkled on the surface thereof, and the inner wax mold (1) is placed in a ventilated environment with a humidity of 50 to 70% and a temperature of 15 to 28° C., and is naturally air-dried to obtain an inner layer shell; The inner shell is immersed in the transition layer slurry for 15 to 30 seconds, then the transition layer refractory sand is evenly sprinkled on the surface, and it is placed in a ventilated environment with a humidity of 50 to 70% and a temperature of 15 to 28°C, and the transition layer shell is obtained after natural air drying; The transition layer shell is immersed in the outer layer slurry for 15 to 30 seconds, then the outer layer refractory sand is evenly sprinkled on its surface, and it is placed in a ventilated environment with a humidity of 50 to 70% and a temperature of 15 to 28° C., and the outer shell is obtained after natural air drying.

5. The method for preparing a riser tube for high temperature alloy according to claim 3, characterized in that: The grouting material described in step 4 is mixed with an inner layer slurry, an outer layer slurry, zircon sand, fine upper sand, coarse upper sand and refractory fiber. The mixing process is: mix the inner layer slurry and the outer layer slurry and stir at a low speed for 5 to 8 minutes, then add zircon sand, fine upper sand, coarse upper sand and refractory fiber in sequence to stir into slurry. When the mixed slurry falls freely, it is in the form of discontinuous flocs, which meets the use requirements.

6. The method for preparing a riser tube for high temperature alloy according to claim 4 or 5, characterized in that: The inner layer slurry includes silica sol, 325 mesh zircon powder, defoamer and wetting agent, wherein: the mass ratio of silica sol to 325 mesh zircon powder is 1:3-4; the defoamer model is FA905, and the dosage accounts for 0.05% of the total mass; the wetting agent model is WET-10S, and the dosage accounts for 0.1% of the total mass.

7. The method for preparing a riser tube for a high temperature alloy according to claim 4 or 5, characterized in that: The outer layer slurry includes silica sol, 200-mesh powder and defoamer, wherein the mass ratio of silica sol to 200-mesh powder is 1:3-4, the defoamer model is FA905, and the amount accounts for 0.05% of the total mass.

8. The method for preparing a riser tube for high temperature alloy according to claim 4, characterized in that: The transition layer slurry includes silica sol, 200-mesh powder and defoamer, wherein the mass ratio of silica sol to 200-mesh powder is 1:3-4, the defoamer model is FA905, and the amount accounts for 0.05% of the total mass.

9. The method for preparing a riser tube for high temperature alloy according to claim 4, characterized in that: The inner layer of refractory sand is 80-120 mesh zircon sand; the transition layer of refractory sand is 30-60 mesh upper sand; and the outer layer of refractory sand is 16-30 mesh upper sand.

10. The method for preparing a riser tube for high temperature alloy according to claim 3, characterized in that: The specific calcination treatment in step 6 is: place the riser tube mold shell in a resistance furnace at 750°C for dewaxing treatment and keep it warm for 1 hour, wait for the wax mold of the inner cavity of the riser tube to be completely removed, heat it to 950°C for pre-sintering for 2 hours, and then sinter it at 1150°C for 4 hours to ceramicize it and cool it with the furnace.