Preparation method of high-yield and high-efficiency dispersion liquid and single-walled carbon nanotube
Through the combination of alcohol solvents, acetylacetone metal compound and sulfur source, floating catalytic method and oxidative acid treatment technology, the problems of structural, purity and size uniformity in single-wall carbon nanotube preparation are solved, achieving efficient and pure Single-wall carbon nanotube preparation enhances its potential in high-tech applications.
Patent Information
- Application Number
- CN202411379024.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
AI Technical Summary
In the preparation of single-wall carbon nanotubes, it is difficult to effectively control structure, purity and dimensional uniformity, and there are difficulties in separation and large-scale production, which affects its wide application in high-tech applications.
Single-walled carbon nanotubes are synthesized by floating catalytic method at high temperature by using alcohol solvents, acetylacetonate metal compounds and sulfur sources, and purified by oxidation and acid treatment to optimize the selection of catalysts and gas carbon sources to improve the Yield and quality.
The yield and quality of single-wall carbon nanotubes are significantly improved, the generation rate and total yield of carbon-based products are enhanced, the formation of carbon impurities is reduced, and the purity and graphitization of carbon nanotubes are improved.
Smart Images

Figure CN119038534A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of single-walled carbon nanotube material preparation, and in particular to a high-yield and high-efficiency dispersion liquid and a method for preparing single-walled carbon nanotubes. Background Art
[0002] Single-walled carbon nanotubes are a type of nanomaterial formed by curling a single layer of carbon atoms into a seamless cylinder in a honeycomb hexagonal lattice structure. Its diameter is usually between 0.4-2nm, and its length can range from hundreds of nanometers to several millimeters, and can even be extended to the centimeter level through specific preparation techniques. Single-walled carbon nanotubes have unique physical and chemical properties, such as extremely high elastic modulus and mechanical strength, excellent electrical and thermal conductivity, and unique electronic properties (for example, depending on the way it is curled, single-walled carbon nanotubes can exhibit metallic or semiconductor properties). These properties make it have a wide range of application potential in nanoelectronics, field effect transistors, sensors, conductive materials, composite material reinforcements, energy storage devices (such as lithium-ion batteries and supercapacitors), and drug delivery. In addition, single-walled carbon nanotubes also have excellent chemical stability and high thermal stability, which enables them to maintain their performance under extreme conditions. The main methods for preparing single-walled carbon nanotubes include arc discharge, laser ablation, and chemical vapor deposition (CVD) technology, among which CVD technology is widely used because of its strong controllability, high yield, and relatively low cost. However, controlling the structure, purity and size uniformity of single-walled carbon nanotubes during the preparation process remains a technical challenge. In addition, the separation, purification and large-scale production of single-walled carbon nanotubes also face certain difficulties, but with the advancement of technology, these problems are gradually being solved, making them promising in future high-tech applications.
[0003] The main methods for preparing single-walled carbon nanotubes are chemical vapor deposition, electrochemical stripping, hydrothermal synthesis, arc discharge and chemical oxidation-reduction. Chemical vapor deposition heats carbon source gas and metal catalyst in a reaction chamber to rearrange and crystallize carbon molecules; electrochemical stripping uses charge transfer between carbon nanotubes and substrates for stripping; hydrothermal synthesis uses appropriate precursors and catalysts under high temperature and high pressure to rearrange carbon molecules to form single-walled carbon nanotubes; arc discharge generates high-energy particles and high-temperature plasma through arc discharge technology to generate single-walled carbon nanotubes; chemical oxidation-reduction converts carbon source substances through appropriate oxidants and reductants.
[0004] Chemical vapor deposition (CVD) is a highly complex and technology-intensive process for preparing single-walled carbon nanotubes (SWCNTs). It uses metal nanoparticles as catalysts to decompose carbon-containing gases (such as methane, acetylene, etc.) into carbon atoms under high temperature. These carbon atoms diffuse on the surface of the catalyst and self-organize in a specific direction to form a single-walled carbon nanotube structure with a nanometer diameter. The entire process involves the selection and preparation of the catalyst, the type and flow rate of the reaction gas, and the precise control of reaction conditions such as temperature and pressure. These factors have a significant impact on the diameter, purity and wall structure of the carbon nanotubes. In addition, after the reaction, a series of post-treatment steps are required to remove excess catalyst particles and other impurities to obtain pure single-walled carbon nanotubes with excellent performance. This nanomaterial has a wide range of application potentials in high-tech fields such as nanoelectronic devices, composite materials, and energy storage devices due to its unique physical and chemical properties. The CVD method has become one of the main methods for industrial production of single-walled carbon nanotubes due to its controllability and high yield. However, it also faces challenges in terms of preparation cost and large-scale application. Summary of the invention
[0005] The present application is made in view of the above-mentioned problems, and its purpose is to have significant advantages in the selection of gaseous carbon sources, the selection of catalysts and the selection of organic solvents, so as to provide a dispersion liquid and a method for preparing single-walled carbon nanotubes that significantly improve the yield and quality of the product.
[0006] The first aspect of the present application provides a high-yield and high-efficiency dispersion liquid, which is composed of an alcohol solvent, an acetylacetone metal compound, a sulfur source and a small amount of water.
[0007] In any embodiment, the alcohol solvent is one or more of n-propanol, n-butanol, n-pentanol, and n-hexanol.
[0008] In any embodiment, the acetylacetonate metal compound is one or more of acetylacetonate iron, acetylacetonate cobalt, and acetylacetonate nickel.
[0009] In any embodiment, the sulfur source is one or more of thiophene, thiophenol, and selenophenephenol.
[0010] In any embodiment, the ratio of the alcohol solvent, the co-catalyst and the acetylacetonate metal compound is 40-70 mL: 1-5 mL: 1-2 g.
[0011] The second aspect of the present application also provides a method for preparing single-walled carbon nanotubes with high yield and high efficiency, comprising the following steps:
[0012] a) preparing a dispersion using an alcohol solvent, an acetylacetonate metal compound, a sulfur source and a small amount of water;
[0013] b) introducing the dispersion into a high-temperature furnace at a specific injection speed, controlling the feed gas speed, and reacting to synthesize single-walled carbon nanotubes by a floating catalytic method at a certain temperature;
[0014] c) The crude product is purified by oxidation and acid treatment.
[0015] In any embodiment, the feed gas is a reducing gas and a protective gas in a 1:1 ratio, the reducing gas is acetylene, and the protective gas is nitrogen.
[0016] In any embodiment, the ratio of the injection rate of the feed liquid to the rate of the feed gas is 20-30 sccm: 1 μL / min.
[0017] In any embodiment, the floating catalytic process is carried out at a temperature of 1100-1400°C.
[0018] In any embodiment, the air oxidation temperature of the crude product is 500-600° C., the air oxidation time is 5-7 hours, and 1000-1500 sccm of CO is introduced to remove iron oxide.
[0019] In any embodiment, the acid-treated solution is one or more of concentrated hydrochloric acid, concentrated sulfuric acid and aqua regia, the stirring temperature during the acid treatment is 120-130° C., the stirring time is 8-9 h, and it is repeated 3-5 times.
[0020] The air oxidation time after each acid solution treatment is 7-10h.
[0021] Beneficial effects of the present application: The present invention adopts a unique combination of alcohol solvents, acetyl metal compounds and co-catalysts to form a dispersion, and uses reducing gas and protective gas with high carbon content and reactivity to achieve the auxiliary growth of single-walled carbon nanotubes; acetyl metal compounds are used as catalysts to increase their solubility and stability in non-polar or weakly polar solvents, while having good reaction selectivity, thereby increasing the generation rate and total yield of carbon-based products; and alcohol solvents with suitable carbon chain lengths are easily decomposed at high temperatures to generate simple small molecules, which reduces the formation of carbon impurities and improves the purity of carbon nanotubes; the high carbon content and reactivity of acetylene gas, as well as its simple and direct decomposition path, significantly increase the yield of the product. Compared with traditional production methods, this invention has significant advantages in the selection of gas carbon sources, catalysts and organic solvents, and ultimately greatly improves the yield and quality of carbon-based products. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The scanning electron microscope image and Raman image of the single-walled carbon nanotube of Example 1 of the present application;
[0023] Figure 2 The scanning electron microscope image and Raman image of the single-walled carbon nanotube of Example 2 of the present application;
[0024] Figure 3 The scanning electron microscope image and Raman image of the single-walled carbon nanotube of Example 3 of the present application;
[0025] Figure 4 The scanning electron microscope image and Raman image of the single-walled carbon nanotube of Example 4 of the present application;
[0026] Figure 5 The scanning electron microscope image and Raman image of the single-walled carbon nanotube of Comparative Example 1;
[0027] Figure 6 The scanning electron microscope image and Raman image of the single-walled carbon nanotube of Comparative Example 2;
[0028] Figure 7 The scanning electron microscope image and Raman image of the single-walled carbon nanotube of comparative example 3;
[0029] Figure 8 The scanning electron microscope image and Raman image of the single-walled carbon nanotube of comparative example 4 are shown. DETAILED DESCRIPTION
[0030] Hereinafter, the embodiments of the method for preparing a high-yield and efficient dispersion and single-walled carbon nanotubes of the present application will be specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0031] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0032] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0033] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0034] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0035] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0036] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0037] The core of the present invention is a unique combination of acetylene gas as a carbon source, alcohols as an organic solvent and acetylacetone metal compound as a catalyst. The high carbon content and reactivity of acetylene gas, as well as its simple and direct decomposition path, significantly improve the yield of the product. At the same time, the acetylacetone metal compound catalyst has good solubility, strong dispersibility and high reaction selectivity, which can further optimize the reaction efficiency and improve the generation rate and total yield of carbon-based products; the acetyl group is a part of an organic compound, which can increase the solubility of certain metal organic compounds in non-polar or weakly polar solvents; the acetyl group can increase the solubility by increasing the overall polarity of the compound and providing possible solvent interaction. In addition, the acetylacetone metal compound has good stability in organic solvents, which helps to maintain its long-term activity and avoids the decline in yield caused by catalyst failure. Alcohol solvents (such as ethanol and isopropanol) are easily decomposed at high temperatures to generate simpler small molecules (such as water and carbon dioxide), and these small molecules will not be deposited on the surface of carbon nanotubes or introduce complex carbon structures, which reduces the possibility of forming carbon impurities. When solvents containing benzene rings (benzene, toluene) are pyrolyzed at high temperatures, they are easy to generate complex fragments rich in carbon (polycyclic aromatic hydrocarbons, graphene fragments), which are more likely to be deposited on the surface of the catalyst growing carbon nanotubes, forming irregular carbon impurities, affecting the purity of carbon nanotubes; and these carbon impurities are more likely to adhere to the tube wall during the production process, and are still difficult to collect after purging with a large amount of gas. Compared with traditional short-chain alcohols such as ethanol, long-chain alcohols are conducive to providing more carbon sources during the growth of single-walled carbon nanotubes; however, alcohols with too long carbon chains have too high boiling points and are not easy to volatilize, and absorb heat during the process of chemical bond breaking, causing the local temperature at the feed port to drop, which may cause the catalyst to generate other carbon impurities in the high temperature zone without being evenly dispersed and given activity. The present invention comprehensively considers the selection of gas carbon sources, catalyst selection, and organic solvent selection, and has significant advantages, which can significantly improve the yield and quality of the product.
[0038] In one embodiment of the present application, the present application proposes a method for preparing purified single-walled carbon nanotubes. The method first includes placing a primary single-walled carbon nanotube raw material containing amorphous carbon in air for oxidation treatment at a certain temperature and time to remove the amorphous carbon on the surface. Secondly, the oxidized single-walled carbon nanotubes are mixed with an acid solution under the same or appropriate temperature conditions, and stirred for a certain time and temperature to remove the metal impurities therein. This process needs to be repeated 2-3 times to ensure that the impurities are fully removed. The single-walled carbon nanotubes prepared by this method have been tested by Raman spectroscopy and shown that their degree of graphitization is significantly improved.
[0039] A method for preparing single-walled carbon nanotubes with high yield and high efficiency comprises the following steps:
[0040] a) preparing a dispersion using an alcohol solvent, an acetylacetonate metal compound, a sulfur source and a small amount of water;
[0041] b) introducing the dispersion into a high temperature furnace at a specific injection speed, controlling the feed gas speed, and reacting at a temperature of 1100-1350° C. by a floating catalytic method to synthesize single-walled carbon nanotubes;
[0042] c) The crude product is purified by oxidation and acid treatment.
[0043] In the process of preparing single-walled carbon nanotubes, alcohol solvents are used as carbon sources, co-catalysts enhance catalyst activity to promote growth, and acetyl metal compounds are used as catalyst precursors to generate key catalyst particles. The synergistic effect of the three optimizes the preparation process and quality of carbon nanotubes. However, the specific synergistic mechanism depends on many factors such as the type, proportion and reaction conditions of solvents, co-catalysts, and acetyl metal compounds.
[0044] Under the condition of reaction temperature above 1000 degrees Celsius, after the dispersion enters the reactor, the iron atom group enters the reactor during the dispersion process of the alcohol reagent, and at this time, the sulfur in the co-catalyst is wrapped around the outside of the iron atom group to form an S-Fe-S core-shell structure. The thickness of the S shell depends on the amount of co-catalyst added, and the alcohol reagent, as a carbon source, grows along the end of Fe under the action of S.
[0045] Specifically, the alcohol solvent is one or more of n-propanol, n-butanol, n-pentanol and n-hexanol.
[0046] Specifically, the acetylacetonate metal compound is one or more of ferric acetylacetonate, cobalt acetylacetonate, and nickel acetylacetonate. More preferably, the acetylacetonate metal compound is ferric acetylacetonate.
[0047] Iron acetylacetonate is more stable than nickel acetylacetonate and cobalt acetylacetonate in the preparation of this application. Nickel and cobalt atoms are more active and more prone to redox reactions. In addition, nickel acetylacetonate and cobalt acetylacetonate are more likely to produce a large amount of multi-walled carbon nanotubes in the process of producing single-walled carbon nanotubes, affecting the purity of the product.
[0048] Specifically, the co-catalyst is one or more of thiophene, thiophenol, and selenophenephenol.
[0049] In the co-catalyst, sulfur in thiophene and thiophenol is wrapped around the outside of the iron atom group to form an S-Fe-S core-shell structure. The thickness of the S shell depends on the amount of co-catalyst added, and the alcohol reagent, as a carbon source, grows along the end of Fe under the action of S. In addition, selenium, which is in the same main group as sulfur, also acts as a co-catalyst, and the chemical reaction activity of selenium is greater than that of sulfur. Therefore, selenol also acts as a co-catalyst in the process of preparing single-walled carbon nanotubes.
[0050] Specifically, the ratio of the alcohol solvent, the co-catalyst and the acetylacetone metal compound is 40-70 mL: 1-5 mL: 1-2 g.
[0051] The amount of alcohol solvent, co-catalyst and acetyl metal compound used will have a significant impact on the preparation results.
[0052] Alcohol solvents: Mainly used to adjust the dilution and concentration of active species in the reaction mixture. If too much is added, the reaction mixture will be too dilute, reducing the contact frequency between the reaction molecules, which may affect the formation of carbon nanotubes. If too little is added, the reaction may be too concentrated, and the heat generated cannot be dissipated in time, which may cause the reaction to get out of control or affect the structure and properties of carbon nanotubes.
[0053] Catalyst: Increase the reaction speed and efficiency. If too much is added, the reaction speed can be increased, but it may also cause the reaction to get out of control and even affect the quality of carbon nanotubes. If too little is added, the reaction may be slow, thus affecting the efficiency of single-walled carbon nanotube production.
[0054] Acetyl metal compound: as a metal catalyst. If too much is added, it may affect the purity and performance of carbon nanotubes due to the difficulty in removing the metal during the purification process. If too little is added, it may lead to insufficient carbon source, thus affecting the formation of carbon nanotubes.
[0055] Therefore, in actual operation, it is necessary to conduct continuous experiments and verifications, comprehensively consider various factors, and select the appropriate addition amount to ensure the generation efficiency and quality of carbon nanotubes.
[0056] Specifically, the gas feed includes a reducing gas and a protective gas in a ratio of 1:1, the reducing gas is acetylene, and the protective gas is nitrogen.
[0057] Specifically, the ratio of the injection rate of the feed liquid to the injection rate of the feed gas (including the protective gas and the reducing gas in a ratio of 1:1) is 20-30 sccm:1 μL / min.
[0058] Specifically, the single-walled carbon nanotubes are prepared by a floating catalytic method at a temperature of 1100-1400°C.
[0059] Specifically, a method for large-scale preparation of single-walled carbon nanotubes is specifically characterized in that the air oxidation temperature of the crude product is 500-600°C to remove excess amorphous carbon, and 1000-1500sccm of CO is introduced to remove iron oxide.
[0060] Specifically, the air oxidation time of the crude product is 5-7h.
[0061] Specifically, the acid solution used to remove the amorphous carbon is one or more of 3M concentrated hydrochloric acid, concentrated sulfuric acid and aqua regia.
[0062] Specifically, the stirring temperature during the acid solution treatment process for purifying single-walled carbon nanotubes is 120-140° C., and the stirring time is 8-9 hours.
[0063] Stirring is required during the acid treatment process because the single-walled carbon nanotubes are in the form of films and filaments, not powders. Fully stirring during the acid treatment process can make the acid and the single-walled carbon nanotubes contact more evenly.
[0064] Example
[0065] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0066] Embodiment 1:
[0067] 70mL of n-propanol was dissolved and dispersed or dissolved with 1g of ferric acetylacetonate and 2.5mL of thiophene, and highly graphitized single-walled carbon nanotubes were synthesized at 1250°C by floating catalysis in an environment of acetylene and nitrogen. The injection rate of the feed liquid was 50μL / min, and the feed gas was 625sccm of acetylene and 625sccm of nitrogen. First, the crude product was exposed to air for oxidation at 525°C for 5h to remove amorphous carbon on the surface, and 1000sccm of CO was introduced to remove iron oxide. Then, an acid solution was used for stirring at 125°C for 18h, and the process was repeated 2-3 times to remove metal impurities in the crude product. This method produced 1.4026g of single-walled carbon nanotubes in 2h, with excellent quality and a G / D value of up to 210.5.
[0068] Embodiment 2:
[0069] 70mL of n-butanol was dissolved and dispersed or dissolved with 1g of ferric acetylacetonate and 2.5mL of thiophene, and highly graphitized single-walled carbon nanotubes were synthesized at 1250°C by floating catalysis in an environment of acetylene and nitrogen. The injection rate of the feed liquid was 50μL / min, and the feed gas was 625sccm of acetylene and 625sccm of nitrogen. First, the crude product was exposed to air for oxidation at 525°C for 5h to remove amorphous carbon on the surface, and 1200sccm of CO was introduced to remove iron oxide. Then, an acid solution was used for stirring at 125°C for 18h, and the process was repeated 2-3 times to remove metal impurities in the crude product. This method produced 1.9078g of single-walled carbon nanotubes in 2h, with excellent quality and a G / D value of 241.5.
[0070] Embodiment 3:
[0071] 70mL of n-pentanol was dissolved and dispersed or dissolved with 1g of ferric acetylacetonate and 2.5mL of thiophene, and highly graphitized single-walled carbon nanotubes were synthesized at 1250°C by floating catalysis in an environment of acetylene and nitrogen. The injection rate of the feed liquid was 50μL / min, and the feed gas was 625sccm of acetylene and 625sccm of nitrogen. First, the crude product was exposed to air for oxidation at 525°C for 5h to remove amorphous carbon on the surface, and 1500sccm of CO was introduced to remove iron oxide. Then, the acid solution was stirred at 125°C for 18h, and the process was repeated 2-3 times to remove metal impurities in the crude product. This method produced 1.2741g of single-walled carbon nanotubes in 2h, with excellent quality and a G / D value of up to 207.4.
[0072] Embodiment 4:
[0073] 70mL of n-hexanol was dissolved and dispersed or dissolved with 1g of ferric acetylacetonate and 2.5mL of thiophene, and highly graphitized single-walled carbon nanotubes were synthesized at 1250°C by floating catalysis in an environment of acetylene and nitrogen. The injection rate of the feed liquid was 50μL / min, and the feed gas was 625sccm of acetylene and 625sccm of nitrogen. First, the crude product was exposed to air for oxidation at 525°C for 5h to remove amorphous carbon on the surface, and 1350sccm of CO was introduced to remove iron oxide. Then, an acid solution was used for stirring at 125°C for 18h, and the process was repeated 2-3 times to remove metal impurities in the crude product. This method produced 1.1085g of single-walled carbon nanotubes in 2h, with excellent quality and a G / D value of 173.4.
[0074] Comparative Example 1:
[0075] The steps are compared with Example 2, the only difference being that n-butanol is replaced by ethanol. This method produces 0.9826 g of single-walled carbon nanotubes in 2 hours with excellent quality, and the G / D value can reach 147.7.
[0076] Comparative Example 2:
[0077] The steps are compared with Example 2, the only difference being that ferric acetylacetonate is replaced by ferrocene. This method produces 1.1254 g of single-walled carbon nanotubes in 2 hours with excellent quality, and the G / D value can reach 145.1.
[0078] Comparative Example 3:
[0079] The steps are compared with Example 2, the only difference is that 1g of ferric acetylacetonate is replaced by 1.2g of ferric acetylacetonate. This method produces 1.3567g of single-walled carbon nanotubes in 2h with excellent quality, and the G / D value can reach 127.9.
[0080] Comparative Example 4:
[0081] The steps are compared with Example 2, the only difference is that 1g of ferric acetylacetonate is replaced by 0.8g of ferric acetylacetonate. This method produces 1.0259g of single-walled carbon nanotubes in 2h with excellent quality, and the G / D value can reach 114.4.
[0082] Reference Figure 1-8 As shown. The boiling point order of n-propyl alcohol, n-butyl alcohol, n-pentanol and n-hexyl alcohol in embodiment 1-4 is arranged according to molecular weight, and the larger the molecular weight, the higher the boiling point. This is because the intermolecular force is enhanced along with the increase of molecular weight, so that higher temperature (i.e. higher energy) needs to be used to break the intermolecular attraction. But n-propyl alcohol has a shorter carbon chain structure compared to n-butyl alcohol, which just causes the experimental condition that n-propyl alcohol provides less content carbon source to grow single-walled carbon nanotubes.
[0083] In Comparative Example 1, n-butanol was replaced with ethanol, and the unit time yield of single-walled carbon nanotubes decreased. Compared with traditional short-chain alcohols, long-chain alcohols help provide more carbon sources to promote the growth of single-walled carbon nanotubes. However, long-chain alcohols have too high boiling points and are not easily volatile. During the chemical bond breaking process, they absorb heat and cause the local temperature to drop, which may cause the catalyst to generate other carbon impurities in the high temperature area, especially when it is not fully dispersed and activated.
[0084] Comparative Example 2 replaces ferric acetylacetonate with ferrocene, and the unit time yield of single-walled carbon nanotubes decreases. The acetyl group can increase the solubility by increasing the overall polarity of the compound and providing possible solvent interaction. Ferrocene has a certain solubility in organic solvents, but due to its relatively symmetrical structure and lack of polarity, its solubility may be relatively low.
[0085] Comparative Examples 3-4 add too much or too little ferric acetylacetonate and have a significant impact on the output of single-walled carbon nanotubes. The density of the catalyst iron particles will increase, causing them to aggregate into larger particles on the substrate. Such particle size is often not conducive to forming a single-wall structure, and is more inclined to generate multi-walled carbon nanotubes (MWCNTs) or disordered carbon structures. In addition, the excessive use of catalysts may also cause the reaction system to produce excessive carbon particles and unstructured carbon, so the output and purity of single-walled carbon nanotubes can be reduced. If the catalyst is insufficient, the number of catalytic reaction active sites will be reduced, which will directly affect the growth density and output of carbon nanotubes. The number of catalysts is too few, which means that the active centers available for growing carbon nanotubes are insufficient, thereby causing the overall output of single-walled carbon nanotubes to decline.
[0086] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A high-yield, high-efficiency dispersion, It is characterized in that It is composed of an alcohol solvent, an acetylacetone metal compound, a sulfur source and a small amount of water.
2. The dispersion according to claim 1, It is characterized in that The alcohol solvent is one or more of n-propanol, n-butanol, n-pentanol and n-hexanol.
3. The dispersion according to claim 1, It is characterized in that The acetylacetonate metal compound is one or more of acetylacetonate iron, acetylacetonate cobalt, and acetylacetonate nickel.
4. The dispersion according to claim 1, It is characterized in that The sulfur source is one or more of thiophene, thiophenol and selenophenephenol.
5. The dispersion according to claim 1, It is characterized in that The ratio of the alcohol solvent, the co-catalyst and the acetylacetone metal compound is 40-70 mL: 1-5 mL: 1-2 g.
6. A method for preparing single-walled carbon nanotubes with high yield and high efficiency, The following steps are involved: a) preparing a dispersion using an alcohol solvent, an acetylacetonate metal compound, a sulfur source and a small amount of water; b) introducing the dispersion into a high-temperature furnace at a specific injection speed, controlling the feed gas speed, and reacting to synthesize single-walled carbon nanotubes by a floating catalytic method at a certain temperature; c) The crude product is purified by oxidation and acid treatment.
7. The preparation method according to claim 6, It is characterized in that The feed gas is a reducing gas and a protective gas in a ratio of 1:1, the reducing gas is acetylene, and the protective gas is nitrogen.
8. The preparation method according to claim 6, It is characterized in that The ratio of the injection speed of the feed liquid to the speed of the feed gas is 20-30 sccm:1 μL / min.
9. The preparation method according to claim 6, It is characterized in that The floating catalytic method is carried out at a temperature of 1100-1400°C.
10. The preparation method according to claim 6, It is characterized in that The air oxidation temperature of the crude product is 500-600°C, the air oxidation time is 5-7h, and 1000-1500sccm of CO is introduced to remove iron oxide; the acid treatment solution is one or more of concentrated hydrochloric acid, concentrated sulfuric acid and aqua regia, the stirring temperature during the acid treatment process is 120-130°C, the stirring time is 8-9h, and it is repeated 3-5 times.
Citation Information
Patent Citations
Sulfur and nitrogen double doped carbon nano tube film and preparation method thereof
CN110316720A
Mixed carbon nanotube film and preparation method thereof
CN112174114A
Method and device for preparing high-quality single-walled carbon nanotubes
CN118324125A
Method for preparing single-walled carbon nanotube at fixed gas-liquid ratio
CN118419915A
Single-wall carbon nanotube synthesizing process
CN1673073A
Cited By
Process for preparing single-walled carbon nanotubes and graphene by stripping multi-walled carbon nanotubes
CN120483120A